US 4,343,908 AGrant
Optical Glass Having n.sub.D =1.63.+-.(1.5.times.10.sup.-2), v.sub.D =59.5.+-.1.0 With a High Chemical Stability and a Low Tendency to Crystallization
Issue Date:1982-08-10
•10 Claims
Abstract
An optical glass having n.sub.D =1.63.+-.(1.5.times.10.sup.-2), v.sub.D =59.5.+-.1.0, a high chemical stability and a low tendency to crystallization is provided, consisting essentially of (in percent. by weight): wherein the sum of SiO.sub.2 +B.sub.2 O.sub.3 is 50-53, the weight ratio SiO.sub.2 :B.sub.2 O.sub.3 is 0.8-1.0, the sum SrO+BaO is 26-31, and the sum ZnO+La.sub.2 O.sub.3 is 12-17.
Metadata
Assignee
- Schott Glaswerke
Inventors
- Marga Faulstich
- Volmar Geiler
Application Information
Application Number:US 2211106
Filing Date:1980-12-29
Priority Date:1979-12-29
Art Unit:113
Classifications
IPC:
C03C 308
Field of Search:
10650147 Q;5478;903
Patent Drawings
This patent does not have any drawings.
Description
BACKGROUND OF THE INVENTION
The present invention relates to a glass having the optical characteristics n.sub.D =1.630.+-.(1.5.multidot.10.sup.-2) and v.sub.D =59.5.+-.1.0. Glasses having these optical characteristics are known (see for instance DE-PS No. 14 21 877=U.S. Pat. No. 3,248,238), whose disclosures are incorporated by reference herein). However, they all contain a high percentage of BaO and consequently have very little chemical stability.
SUMMARY OF THE INVENTION
Accordingly, it is an object of this invention to provide a glass having the above mentioned optical characteristics, a good chemical stability and, at the same time, such little tendency to crystallization that it can be produced in a crucible melting batch process or in a continuous tank melting process in the form of drops, pressings, billets or glass blocks of any desired shape.
Upon further study of the specification and appended claims, further objects and advantages of this invention will become apparent to those skilled in the art.
These objects have been attained by providing an optical glass having the optical characteristics n.sub.D =1.63.+-.(1.5.times.10.sup.-2), v.sub.D =59.5.+-.1.0, a high chemical stability and a low tendency to crystallization, and having the following composition (in percent. by weight):
DETAILED DISCUSSION
Fully conventional glassmaking procedures can be employed to prepare the glasses of this invention. Advantageously, the mentioned crucible melting batch process (for details, see, e.g. U.S. Pat. No. 3,898,093, whose disclosure is incorporated by reference herein) or the continuous tank melting process (for details, see e.g., U.S. Pat. No. 3,970,466, whose disclosure is incorporated by reference herein), is used. In this regard, reference is made to the following examples.
The glasses of this invention are particularly well adapted for conventional use in objectives for cameras, projectors and similar instruments.
The chemical stabilities, and tendencies to crystallization as measured via the standard methods, disclosed in the examples below, of the glasses of this invention, generally have values of:
Of particular importance is the attainment of the combined properties (a) through (h). It is in this sense that these properties are described as high stability and low crystallization tendency.
Without further elaboration, it is believed that one skilled in the art can, using the preceding description, utilize the present invention to its fullest extent. The following preferred specific embodiments are, therefore, to be construed as merely illustrative, and not limitative of the remainder of the disclosure in any way whatsoever. In the following examples, all temperatures are set forth uncorrected in degrees Celsius; unless otherwise indicated, all parts and percentages are by weight.
EXAMPLE I
Certain embodiments of this invention as well as three known high-barium-content glasses A, B, C are specified by way of example in the accompanying table. Indicative of the actual weight quantities of batch ingredients for each embodiment, are those given below for Example 8 of the table.
Melt Example
(Example 8, see table)
Each of the well mixed batches is introduced at 1300.degree.-1350.degree. C. into a 50 liter Pt-crucible, then heated up to 1370.degree. C. and refined for approximately 5 hrs until bubble-free. The melt is then left to stand at 1300.degree. C. and, at approximately 1150.degree. C., run through a discharge pipe into pre-heated metal molds of the desired form to make billets. Alternatively, the melt is pressed to make drops or pressings. Using a suitable Zac-stone tank it is also possible to produce a melt of the above specified compositions continuously. This can also be processed into billets, drops and pressings as required.
EXAMPLE II
(see Example 5 of the table)
The following describes by way of example an analysis of a glass according to this invention.
This glass has the following properties:
The chemical stability (tested by standard acid resistance-staining and climatic change stability tests as described, for example, in Schott pocket catalogue No. 3050, (1972)) is one class better than that of currently available conventional glasses having these optical characteristics.
The crystallization test (O. H. Grauer and E. H. Hamilton: Improved Apparatus for Determination of Liquidus Temperatures and Rates of Crystal Growth in Glasses; J. Research Natl. Bur. Standards, 44 (5), 495-502 (1950), RP 2096), after tempering for 60 minutes in a gradient furnace, shows no devitrification in the glass, and on the surface, minor surface crystals at 915.degree. C. (corresponding to 1.4.times.10.sup.3 d Pa.s), with a crystal growth rate of 0.1 .mu./min.
EXAMPLE III
(see Example 8 of the table)
The crystallization test after 60 minutes showed no devitrification in the glass, minor devitrification at the surface at 970.degree. C. (corresponding to 250 dPa.s), and a crystal growth rate of 1.2 .mu./min.
The preceding examples can be repeated with similar success by substituting the generically or specifically described reactants and/or operating conditions of this invention for those used in the preceding examples.
From the foregoing description, one skilled in the art can easily ascertain the essential characteristics of this invention, and without departing from the spirit and scope thereof, can make various changes and modifications of the invention to adapt it to various usages and conditions.
Claims
What is claimed is:
1. An optical glass having n.sub.D =1.63.+-.(1.5.times.10.sup.-2), v.sub.D =59.5.+-.1.0, a high chemical stability and a low tendency to crystallization, and consisting of (in percent. by weight): SiO.sub.2 23-27 B.sub.2 O.sub.3 24-30 SrO 18-31 La.sub.2 O.sub.3 10-16 Al.sub.2 O.sub.3 2-4 BaO 0-10 CaO 0-5 ZnO 0-6 Y.sub.2 O.sub.3 0-5 ZrO.sub.2 0-2 Li.sub.2 O, Na.sub.2 O and/or K.sub.2 O 0-1.5 As.sub.2 O.sub.3 and/or Sb.sub.2 O.sub.3 0-1 F and/or Cl 0-1, wherein the sum of SiO.sub.2 + B.sub.2 O.sub.3 is 50-53, the weight ratio SiO.sub.2 :B.sub.2 O.sub.3 is 0.8-1.0, the sum SrO + BaO is 26-31, and the sum ZnO + La.sub.2 O.sub.3 is 12-17. ______________________________________
2. An optical glass of claim 1 having the following properties: range ______________________________________ chemical stability (a) acid class, class f better than 5c (b) erosion of 0.1.mu. in min. in more than 6 min. standard acetate, pH 4.5 (c) stain test class F1 3-4 (d) thickness of layer <0.24 destroyed after 1 hour in a solution, pH 5.6 (e) climatic change better than stability after 30 hrs class 4 (f) stray light .ltoreq.4.5% crystallization tendency (g) essentially no devitrification (h) crystal growth rate of .ltoreq.1.2 .mu./min. ______________________________________
3. An optical glass of claim 1 having the following property: acid class, class f: better than 5c.
4. An optical glass of claim 1 having the following property: erosion of 0.1.mu. m in min. in standard acetate, pH 4.5.: more than 6 min.
5. An optical glass of claim 1 having the following property: stain test class Fl: 3-4.
6. An optical glass of claim 1 having the following property: thickness of layer destroyed after 1 hour in a solution, pH 5.6: <0.24.
7. An optical glass of claim 1 having the following property: climatic change stability after 30 hours: better than class 4.
8. An optical glass of claim 1 having the following property: stray light: .ltoreq.4.5%.
9. An optical glass of claim 1 having essentially no devitrification.
10. An optical glass of claim 1 having a crystal growth rate of .ltoreq.1.2 .mu./min.
Patent Citations (5)
| Patent | Date | Inventor | Cited By |
|---|---|---|---|
| US3248238 | 1966-04-01 | Faulstich | |
| US3529980 | 1970-09-01 | Bromer et al. | |
| US3898093 | 1975-08-01 | Faulstich et al. | |
| US3970466 | 1976-07-01 | Faulstich | |
| JPX54-003115 | 1979-01-01 |