US 6,274,932 B1Grant
Semiconductor device having metal interconnection comprising metal silicide and four conductive layers
Issue Date:2001-08-14
•14 Claims
•6 Drawing Sheets
Abstract
A semiconductor device having a metal interconnection includes an insulating film provided on a semiconductor substrate via a diffusion layer. An interlayer contact hole is formed in the insulating film. A metal silicide layer is provided at the bottom of the interlayer contact hole. A first conductive film comprises a single or a plurality of metal films provided on the insulating film and the interlayer contact hole. A second conductive film is provided in the interlayer contact hole. A third conductive film is provided on the first conductive film and the second conductive film. A fourth conductive film is provided on the third conductive film. This semiconductor device has improved durability with respect to electromigration or stress migration. Even when the interconnection has a multilevel structure, the contact resistance can be reduced by causing the interlayer contact hole portions to contact one another by the same kind of metal.
Metadata
Assignee
- NEC Corporation
Inventor
- Kaoru Mikagi
Application Information
Application Number:US 08/520,003
Filing Date:1995-08-28
Priority Date:1994-08-30
Art Unit:7
Classifications
IPC:
H01L 2945H01L 214763H01L 21441
Field of Search:
257754257750
Patent Drawings (6 sheets)
Description
BACKGROUND OF THE INVENTION
[0002] 1. Field of the Invention
[0003] The present invention relates to a semiconductor device having a metal interconnection.
[0004] 2. Description of the Related Art
[0005] Some of known conventional semiconductor devices are disclosed in U.S. patent application Ser. Nos. 4,789,648 and 4,944,836. The first conventional semiconductor device will be described with reference to FIGS. 1A and 1B and the second conventional semiconductor device will be described with reference to FIGS. 2A to 2E.
[0006] (a) First Conventional Semiconductor Devices
[0007] First, the semiconductor device described in U.S. patent application Ser. No. 4,789,648 (hereinafter called the “first prior art example”) will be discussed with reference to FIGS. 1A and 1B. FIGS. 1A and 1B are vertical crosssectional views illustrating the fabrication process for this semiconductor device (first prior art example) consisting of steps 1A and 1B.
[0008] According to the first prior art example, as shown in FIG. 1A, an insulating film 104aas a silicon dioxide film is formed on a silicon substrate 101 by chemical vapor deposition (hereinafter referred as CVD) or the like, a groove pattern is formed by known techniques, and then an aluminum film (Al film) 114 as a conductive film is formed by sputtering.
[0009] At this time, the thickness of the insulating film 104ais set equal to the thickness of the necessary interconnection film plus the thickness of the conductive film. A silicon nitride which serves as a stopper at the later step of polishing the metal film may be formed on the insulating film 104a.
[0010] Subsequently, the Al film 114 is polished and removed by chemical-mechanical polishing (hereinafter called “CMP”) using a slurry consisting of alumina (Al2O3)-added deionized water or an Al2O3-added nitrate solution, yielding a groove interconnection structure which has a groove pattern filled with an interconnection material (Al film 114), as shown in FIG. 1B.
[0011] (b) Second Conventional Semiconductor Devices
[0012] Next, the semiconductor device described in U.S. patent application Ser. No. 4,944,836 (hereinafter called the “second prior art example”) will be discussed with reference to FIGS. 2A to 2E. FIGS. 2A-2E are vertical cross-sectional views illustrating the fabrication process for this semiconductor device (second prior art example) consisting of steps A to E.
[0013] According to the second prior art example, as shown in FIG. 2A, an insulating film 104aand an underlying Al interconnection 112 are formed using known techniques, an insulating film 104b(which may be a silicon dioxide film) is formed on the surface of the resultant structure, and a stopper 113 of Al2O3is then formed in a predetermined region by lithography, etching and the like.
[0014] Then, an insulating film 104cas a silicon dioxide film is formed on the stopper 113 and the insulating film 104b, as shown in FIG. 2B.
[0015] Next, as shown in FIG. 2C, the insulating film 104cand insulating film 104bare patterned by selective etching using a resist (not shown) as a mask to form an interlayer contact hole 105 which reaches the underlying Al interconnection 112.
[0016] As the stopper 113 is not etched at this time, only that portion of the insulating film 104bwhich lies under the opening of the stopper 113 is removed.
[0017] Subsequently, an Al film 114 is formed on the entire surface as shown in FIG. 2D by a known method like sputtering.
[0018] Then, the Al film 114 is polished and removed by CMP, yielding a groove interconnection structure which has the Al-filled interlayer contact hole 105 and an Al-filled groove pattern, as shown in FIG. 2E.
[0019] (c) Third Conventional Semiconductor Devices
[0020] Another known conventional semiconductor device is described in “Proceedings of 1993 VLSI Multilevel Interconnection Conference, pp. 15-21 (1993)” (hereinafter called the “third prior art example”). This third prior art example will now be discussed with reference to FIGS. 3A to 3E, which are vertical cross-sectional views illustrating the fabrication process for this example.
[0021] According to the third prior art example, as shown in FIG. 3A, first, an insulating film 104aof PI 5180 (polyimide resin) is formed 500 to 1000 nm thick on a silicon substrate 101 by rotational coating.
[0022] Next, a stopper 113 is formed of a silicon nitride film on the top of this insulating film 104aby a plasma CVD technique.
[0023] Then, a photoresist 116 to be an etching mask is formed in a predetermined region as shown in FIG. 3B using a lithography technique.
[0024] As shown in FIG. 3C, the stopper 113 and the insulating film 104aare etched by reactive ion etching using this photoresist 114 as a mask, forming a groove pattern for interconnection. Then, the photoresist 116 is removed.
[0025] Next, as shown in FIG. 3D, a tantalum film (Ta film) 106ais formed by sputtering, followed by the formation of a copper film (Cu film) 109aon the Ta film 106ato bury the interconnection groove pattern.
[0026] Then, as shown in FIG. 3E, the Cu film 109aand the Ta film 106aare removed by a known CMP process called “Damascene process ” in such a way that the Cu film 109aand Ta film 106aremain only inside the interconnection groove pattern. At this time, the stopper 113 serves as a stopper layer in the polishing step because the polishing speed of the stopper 113 on the insulating film 104ais slower than those of the Cu film 109aand Ta film 106a.
[0027] According to the third prior art example, a semiconductor device having an interconnection whose main conductive layer is made of Cu is fabricated through those steps A to E.
[0028] (d) Fourth Conventional Semiconductor Devices
[0029] A further known conventional semiconductor device is described in Unexamined Japanese Patent Publication No. Sho 63-207153 (hereinafter called the “fourth prior art example”). This example will now be discussed with reference to FIGS. 4A to 4F which are vertical cross-sectional views illustrating the fabrication process consisting of steps 4A to 4B.
[0030] According to the fourth prior art example, as shown in FIG. 4A, an insulating film 104aconstituted of a silicon dioxide film is formed on a silicon substrate (not shown).
[0031] Subsequently, an underlying Al interconnection 112 of 1.0 μm in thickness is formed using a known technique, and an insulating film 104bconstituted of a PSG film with a thickness of 1.0 to 1.5 μm is formed on the entire surface of the resultant structure.
[0032] Then, an upper lying Al interconnection 115 having a thickness of 1.0 μm is formed on the insulating film 104bas shown in FIG. 4B.
[0033] Next, as shown in FIG. 4C, a stopper 113 made of a silicon nitride film of 200 nm thick is formed on the entire surface of the resultant structure by a plasma CVD technique.
[0034] Subsequently, the stopper 113, the upper lying Al interconnection 115 and the insulating film 104bare partially removed using a resist (not shown) as an etching mask to form an interlayer contact hole 105 in the portion where the underlying Al interconnection 112 crosses the upper lying Al interconnection 115, as shown in FIG. 4D.
[0035] Single positioning is sufficient for opening this hole, and the opening need not be made particularly narrow and should have a diameter about the same as the widths of those interconnections. Therefore, the precision of the positioning need not be particularly high.
[0036] Next, an Al film 114 is formed 2000 to 3000 nm thick by downflow vapor deposition, as shown in FIG. 4E.
[0037] Then, the Al film 114 on the stopper 113 is polished out, yielding a structure with the Al film 114 buried in the interlayer contact hole 105, as shown in FIG. 4F.
[0038] The first to fourth prior art examples have the following shortcomings.
[0039] For the first prior art example (the semiconductor device disclosed in U.S. patent application Ser. No. 4,789,648), the point of exposure of the insulating film 104ain the CMP process is the end of the polishing (see FIG. 1B). It is therefore easy to detect the end by a change in electric capacitance.
[0040] The interconnection itself has a single-layer structure of Al (Al film 114 or Al alloy) so that a contact with the same kind of metal is made at the interlayer contact portion, resulting in a low contact resistance. But, this first prior art example suffers poor durability with respect to electromigration and stress migration.
[0041] The interconnection itself of the first prior art example cannot therefore have high and continuing reliability.
[0042] Even if one tries to use a metal, such as Cu or Au, which has a high conductivity and high durability with respect to the electromigration and stress migration to overcome this problem, those metals are difficult to use due to their reaction with silicon dioxide film and their adhesion to insulating film.
[0043] For the second prior art example (the semiconductor device disclosed in U.S. patent application Ser. No. 4,944,836), like the first prior art example, the point of exposure of the insulating film in the metal CMP process is the end of the polishing. It is therefore easy to detect the end by a change in electric capacitance.
[0044] While the interconnection itself has a single-layer structure of Al film or Al alloy so that a contact with the same kind of metals is made at the interlayer contact portion, resulting in a low contact resistance, this second prior art example suffers poor durability with respect to electromigration and stress migration as per the first prior art example.
[0045] In the second prior art example, metal like Cu which reacts with the silicon dioxide film or Au which has poor adhesion with the insulating film cannot be used as an interconnection material.
[0046] Further, the structure and process of this example are such that although the stopper used in the polishing process is Al2O3having a high dielectric constant (see “the stopper 113 formed of Al2O3” in FIG. 2A), it remains after the formation of the interconnection, thus increasing the interlayer capacitance. This results in lower electrical performance.
[0047] The third prior art example employs such an interconnection structure that the Ta film 106aprotects the Cu film 109a(see FIG. 3E), thus ensuring a high durability with respect to electromigration and stress migration.
[0048] Further, when Ta as a barrier metal is also removed by polishing, it is easy to detect the end of the polishing.
[0049] According to the third prior art example, however, when the interconnection takes a multilevel structure, the interlayer contact hole portion provides a contact with different metals, namely, Cu as a conductive film lying over the lower multilevel interconnection and Ta as a conductive film underlying the upper multilevel interconnection. As a result, the contact resistance becomes higher than the case of the Cu—Cu contact, also increasing the overall electric resistance of the multilevel interconnection, so that the obtained semiconductor device does not have good electrical characteristics.
[0050] To form the structure that provides a contact with the same kind of metal at the interlayer contact portion, it is necessary to leave the Ta film 106ain the polishing process and then form the Cu film 109athereon to provide the interconnection in the third prior art example (see FIGS. 3D and 3E). With Ta left as in this case, the end of the polishing cannot be detected.
[0051] In the fourth prior art example (the semiconductor device disclosed in Unexamined Japanese Patent Publication No. Sho 63-207153), the point of exposure of the insulating film in the CMP process for the metal film is the end of the polishing, so that it is easy to detect the end by a change in electric capacitance.
[0052] As in the first and second prior art examples, however, the interconnection itself has a single-layer structure of Al (Al film 114 or Al alloy) (see FIG. 4F). While the same kind of metals contact with each other at the interlayer contact portion, resulting in a low contact resistance, this fourth prior art example also suffers poor durability with respect to electromigration and stress migration.
[0053] In the fourth prior art example, at the time of forming the interlayer contact hole, a hole of approximately the same width as the interlayer contact hole is formed so that the opening need not be made particularly narrow (see FIG. 4D). If positioning with the positioning pattern is inaccurate, however, the insulating film on the sides of the underlying interconnection is etched so that this etched portion is also filled with metal.
[0054] When fine interconnections with a small positioning margin and a narrow interconnection pitch are to be formed, shorting between the interconnections is likely to occur, thus making it difficult to adapt this example to a semiconductor device which has fine design rules.
[0055] Further, the structure and process of this fourth example are such that a silicon nitride film having a high dielectric constant is used as the stopper 113 in the polishing process and the stopper 113 remains after the formation of the interconnection (see FIG. 4F), thus increasing the interlayer capacitance. The resultant semiconductor device does not have excellent electric characteristics.
SUMMARY OF THE INVENTION
[0056] Accordingly, it is the primary object of the present invention to provide a semiconductor device having a metal interconnection, which overcomes the above-described shortcomings and disadvantages of the first to fourth prior art examples.
[0057] It is the second object of this invention to provide a semiconductor device which is highly durable with respect to electromigration and stress migration and has high and long-lasting reliability.
[0058] It is the third object of this invention to a semiconductor device which employs such a structure as to allow metals of the same kind to contact each other at the interlayer contact hole portion, thus reducing the contact resistance.
[0059] It is the fourth object of this invention to a semiconductor device which permits the end of the polishing process to be precisely detected in the fabrication of an interconnection metal and which has stable electric characteristics and a high yield at the time of fabrication.
[0060] To achieve the above objects, according to one aspect of this invention, there is provided a semiconductor device having a metal interconnection that includes:
[0061] an insulating film provided on a semiconductor substrate via a diffusion layer;
[0062] an interlayer contact hole formed in the insulating film;
[0063] a metal silicide layer provided at a bottom of the interlayer contact hole;
[0064] a first conductive film having a single or a plurality of metal films provided on the insulating film and the interlayer contact hole;
[0065] a second conductive film provided in the interlayer contact hole;
[0066] a third conductive film provided on the first conductive film and the second conductive film; and
[0067] a fourth conductive film provided on the third conductive film.
[0068] According to another aspect of this invention, there is provided a semiconductor device having a metal interconnection, which device comprises:
[0069] an insulating film provided on a semiconductor substrate via a diffusion layer;
[0070] an interlayer contact hole formed in the insulating film;
[0071] a metal silicide layer provided at a bottom of the interlayer contact hole;
[0072] a first conductive film having a single or a plurality of metal films provided on the insulating film and the interlayer contact hole;
[0073] a second conductive film provided in the interlayer contact hole;
[0074] a third conductive film provided on the first conductive film and the second conductive film; and
[0075] a fourth conductive film provided on the third conductive film.
[0076] According to the present invention, the semiconductor device embodying this invention has an interconnection structure having high electric conductivity and high durability against electromigration and stress migration, and has an interconnection which is protected against oxidation and corrosion by a high melting-point metal and silicon nitride film.
[0077] Further, even when the interconnection has a multilevel structure, the same kind of metals contact each other at the interlayer contact hole portion, thus reducing the contact resistance. This interconnection therefore has improved electric characteristics and improved and continuing reliability than the conventional one.
[0078] Furthermore, according to the semiconductor device of this invention, the end of the polishing process can be precisely detected in the fabrication of the interconnection metal, thus ensuring stable electric characteristics and a high yield at the time of fabrication.
BRIEF DESCRIPTION OF THE DRAWINGS
[0079] FIGS. 1A and 1B are vertical cross-sectional views for explaining the first prior art example, illustrating the two-step fabrication process for this prior art example;
[0080] FIGS. 2A through 2E are vertical cross-sectional views for explaining the second prior art example, illustrating the five-step fabrication process for this prior art example;
[0081] FIGS. 3A through 3E are vertical cross-sectional views for explaining the third prior art example, illustrating the five-step fabrication process for this prior art example;
[0082] FIGS. 4A through 4F are vertical cross-sectional views for explaining the fourth prior art example, illustrating the six-step fabrication process for this prior art example;
[0083] FIGS. 5A through 5F are vertical cross-sectional views for explaining a semiconductor device according to a first embodiment of this invention, illustrating the six-step fabrication process for this semiconductor device; and
[0084] FIGS. 6A through 6E are vertical cross-sectional views for explaining a semiconductor device according to a second embodiment of this invention, illustrating the five-step fabrication process for this semiconductor device.
DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0085] Preferred embodiments of the present invention will now be described with reference to the accompanying drawings.
[0086] This invention is not limited to the embodiments to be described below, but may be embodied in various other forms without departing from the scope and spirit of the invention.
First Embodiment
[0087] FIGS. 5A through 5F are vertical cross-sectional views illustrating the step-by-step (six steps) fabrication process for the first embodiment of this invention. In the first embodiment, known techniques such as selective oxidation and ion implantation are used to form a field oxide film 102 and a diffusion layer 103 on a silicon substrate 101 as shown in FIG. 5A.
[0088] Next, an insulating film 104aof a silicon dioxide film having a thickness of about 1000 nm is formed on the top of the resultant structure by thermal CVD using monosilane (SiH4) as the source.
[0089] In this case, the insulating film 104ashould not necessary have a single-layer structure of a silicon dioxide film, but may be a PSG film or BPSG film containing phosphorus (P) or boron (B) or may take a multilayer structure consisting of a silicon dioxide film and a PSG film or a silicon dioxide film and a BPSG film.
[0090] Next, an interlayer contact hole 105 reaching the diffusion layer 103 is formed by reactive ion etching using a photoresist (not shown) as a mask, followed by the removable of this photoresist (FIG. 5A).
[0091] As shown in FIG. 5B, a Ta film 106aas the first conductive film is formed 50 to 150 nm thick by D.C. magnetron sputtering under the conditions of the pressure of 2 to 10 mTorr and the RF power of 1.0 to 5.0 KW.
[0092] Then, the resultant structure is subjected to a heat treatment at 600 to 800° C. for 10 to 30 seconds by the rapid heating using a lamp under the non-oxidation atmosphere of nitride (N2) or argon (Ar), allowing the diffusion layer 103 to react with the Ta film 106aand thus forming a silicide film 107 at the interface between the diffusion layer 103 and Ta film 106a(see FIG. 5B).
[0093] This silicide film 107 is formed to reduce the contact resistance of the diffusion layer 103 and the Ta film 106aas the first conductive film.
[0094] The Ta film 106aas the first conductive film is formed to (1) prevent Cu in a Cu film 109a(see FIG. 5C), which is to be formed on the overlying layer in a later process, from being diffused into the diffusion layer 103, (2) improve the adhesion between the Cu film 109aand the silicon dioxide film (insulating film 104a) as the base insulating film, and (3) improve the durability of the whole interconnection against electromigration and stress migration.
[0095] Although the Ta film 106ais used as the first conductive film in the first embodiment, other metals than Ta, such as tungsten (W), molybdenum (Mo), titanium (Ti), zirconium (Zr), hafnium (Hf), vanadium (V), niobium (Nb), chromium (Cr), osmium (Os), cobalt (Co), iridium (Ir), nickel (Ni), palladium (Pd) and platinum (Pt), and alloys containing those elements may also be used.
[0096] Next, an insulating film mask 108 of a silicon dioxide film is formed by a known plasma CVD technique using SiH4and dinitrogen monoxide (N2O) as a reaction gas, as shown in FIG. 5C.
[0097] This insulating film mask 108 is formed by first forming an insulating film of a silicon dioxide film 200 to 500 nm thick under the conditions of 100 to 300 sccm of SiH4,500 to 1500 sccm of N2O, the substrate temperature of 300 to 400° C., the pressure of 0.25 to 5.0 Torr and the RF power of 0.25 to 2 KW, and then removing the unnecessary portions by known lithography and dry etching techniques.
[0098] The insulating film mask 108 of the silicon dioxide film serves as a stopper layer in polishing the Cu film 109ain the later process (FIG. 5D) which will be discussed in detail later, and also as an end detecting film.
[0099] Subsequently, the Cu film 109aas the second conductive film is formed 200 to 1000 nm thick on the Ta film 106aand insulating film mask 108 by known Cu-CVD (Cu-Chemical Vapor Deposition) (FIG. 5C).
[0100] The Cu-CVD for forming the Cu film 109ais executed by using as a reaction source gas a compound such as hexafluoroacetylacetonato copper(I) vinyltrimethylsilane (hereinafter abbreviated as “(hfa)Cu(vtms)”) or copper bis hexafluoroacetylacetonato (hereinafter abbreviated as “Cu(hfa)2”) which has a low decomposition temperature and provides high vapor pressure even at a relatively low temperature, or using hydrogen (H2) or argon (Ar) as a carrier gas, at the temperature of 100 to 300° C. and under the pressure of 0.5 to 20 Torr.
[0101] At this time, when the diameter of the interlayer contact hole 105 (see FIG. 5A) is very small, a void may be formed in the interlayer contact hole 105 if the step coverage of the Cu film 109ais poor. It is therefore necessary to execute Cu-CVD under the conditions in which the Cu film 109aexhibits a good step coverage.
[0102] When (hfa)Cu(Vtms) or Cu(hfa)2is used as the source, the Cu film 109aif grown at a relatively low temperature can have an excellent step coverage. According to the first embodiment, therefore, Cu-CVD can be carried out at a relatively low temperature of 100 to 300° C. as mentioned above, preferably at 150 to 200° C.
[0103] Although the Cu film 109a(see FIG. 5C) is used as the second conductive film in the first embodiment, besides Ca, aluminum (Al) or an Al-based alloy, gold (Au), copper (Cu) and silver (Ag) or an alloy containing any of the mentioned metals may also be used.
[0104] Next, as shown in FIG. 5D, the Cu film 109aand the insulating film mask 108 are polished and removed the Damascene technique, which is one of the CMP techniques, thereby yielding the structure which has the interlayer contact hole 105 filled with the Cu film 109aand has the Ta film 106aexposed at the surface.
[0105] At this time, a slurry of pure water to which Al2O3particles have been added is used as a polisher, and the conditions such as the rotational polishing speed and applying load are varied depending on the material to be polished and the polishing amount.
[0106] Since the end of polishing is detected by a change in electric capacitance of the polished surface in the ordinary CMP technique, the conventional methods have difficulty in finely detecting the polishing end.
[0107] According to the first embodiment of this invention, however, because of the presence of the insulating film mask 108 under the Cu film 109a(see FIG. 5C), the electric capacitance temporarily increases when the Cu film 109ais polished to expose the insulating film mask 108, and the electric capacitance rapidly decreases when the insulating film mask 108 is completely polished. By detecting this change in electric capacitance, it is very easy to grasp the polishing stage of the Cu film 109aand detect the end of polishing.
[0108] According to the first embodiment, therefore, the polishing can be stopped the instance the Ta film 106ais exposed, preventing the Ta film 106afrom being removed. That is, this embodiment can effect polishing with higher controllability than the prior art methods.
[0109] Although a silicon dioxide film is used as the insulating film mask 108 in the first embodiment as mentioned earlier, this mask should not necessarily be a silicon dioxide film, but may be a silicon nitride film, silicon oxide nitride film or a polyimide resin film which can provide an electric capacitance.
[0110] As shown in FIG. 5E, a Cu film 109bas the third conductive film is formed 250 to 500 nm thick by D.C. magnetron sputtering under the conditions of the pressure of 2 to 10 mTorr, the RF power of 1.0 to 5.0 KW, and the substrate temperature of 200 to 400° C., followed by the formation of a Ta film 106bas the fourth conductive film 20 to 500 nm thick on the top of the resultant structure.
[0111] The Cu film 109bas the third conductive film will serve as the main conductive film of the interconnection that connects semiconductor devices, and is formed of the same metal as the Cu film 109aas the second conductive film in the first embodiment.
[0112] The Ta film 106bas the fourth conductive film is formed to (1) prevent Cu in a Cu film 109bas the third conductive film from being oxidized or corroded, (2) prevent the reaction with the overlying insulating film and improve the adhesion with that insulating film, and (3) improve the durability of the whole interconnection against electromigration and stress migration. In the first embodiment, the Ta film 106bis formed of the same metal as the Ta film 106aas the first conductive film.
[0113] Next, an etching mask 110 made of a silicon nitride film is formed 200 to 400 nm thick on the Ta film 106aunder the conditions of 100 to 300 sccm of SiH4,200 to 1200 sccm of ammonia (NH3), the substrate temperature of 300 to 400° C., the pressure of 0.25 to 5.0 Torr and the RF power of 1.0 to 4.0 KW, and then the unnecessary portions are removed to yield the patterned interconnection by known lithography and dry etching techniques (see FIG. 5E).
[0114] Then, as shown in FIG. 5F, the Ta film 106b, the Cu film 109band the Ta film 106aare sequentially etched to pattern the interconnection by the reactive ion etching using silicon tetrachloride (SiCl4), chlorine (Cl2), NH3and N2under the conditions of the temperature of 280° C., the pressure of 2 Pa, 20 sccm of SiCl4, 20 sccm of Cl2, 10 to 30 sccm of NH3, 80 sccm of N2, and the RF power of 200 KW.
[0115] At this time, a product whose composition is close to that of the silicon nitride film produced during the etching reaction adheres to the side walls of the interconnection and this product serves to prevent side etching and corrosion.
[0116] Because the interlayer contact hole and the interconnection are connected by the same kind of metal in the semiconductor device according to the first embodiment fabricated by the above-described processes, the contact resistance between the contact hole and the interconnection is lower than that of conventional semiconductor devices, thus ensuring excellent electric characteristics.
[0117] Because the Ta film having a high melting point is located above and under the interconnection and the product whose composition is close to that of the silicon nitride film is present on the side walls of the interconnection in the semiconductor device of first embodiment, the oxidation and corrosion of the Cu film as the main conductive film can be suppressed, thus allowing the interconnection to have high and continuing reliability.
[0118] Further, the groove-buried interconnection facilitates making the interconnection thicker, and it is easy to reduce its resistance.
[0119] The semiconductor device of the first embodiment can be adapted for various kinds of semiconductor devices, such as MOS transistors and bipolar transistors, as well as various circuits like memory and logic. This invention therefore includes various kinds of semiconductor devices and circuits and are not limited to any particular type.
[0120] FIGS. 6A through 6E are vertical cross-sectional views for explaining a semiconductor device according to the second embodiment of this invention, illustrating the step-by-step (five steps) fabrication process for this semiconductor device.
[0121] According to the second embodiment, a silicon substrate 101, a field oxide film 102, a diffusion layer 103 and an insulating film 104aare formed first, and then a interlayer contact hole 105 reaching the diffusion layer 103 via the insulating film 104ais formed, as shown in FIG. 6A. Those are formed by using the same techniques, methods and materials as used in the first embodiment.
[0122] Next, a Ta film 106aas the first conductive film is embodiment.
[0123] Next, a Cu film 109aas the second conductive film is formed 200 to 500 nm thick on the Ta film 106aand the insulating film mask 108 by D.C. magnetron sputtering under the conditions of the substrate temperature of 450 to 600° C., the pressure of 2 to 10 mTorr and the RF power of 3.0 to 8.0 KW (FIG. 6A).
[0124] Although the Ta film 106aand the Cu film 109aare used in the second embodiment, metals other than tantalum (Ta), such as tungsten (W) and molybdenum (Mo), may be used, and other metals than copper (Cu), such as aluminum (Al) or an Al-based alloy and gold (Au), may be used as well.
[0125] As shown in FIG. 6B, a heat treatment is performed at 50 to 700° C. for 30 to 120 seconds without breaking the vacuum condition at the time of sputtering the Cu film, thereby causing the Cu film 109ato flow to fill up the interlayer contact hole 105. At this time, the Ta film 106areacts with the diffusion layer 103 to form a silicide film 107.
[0126] As the sputtering employed in the second embodiment has a poorer step coverage than the Cu-CVD technique used in the first embodiment, the filling factor of the Cu film 109ainto the interlayer contact hole 105 becomes lower. But, the vacuum heat treatment allows the Cu film 109ato sufficiently fill up the interlayer contact hole 105.
[0127] Next, as shown in FIG. 6C, the Cu film 109aand the insulating film mask 108 are polished and removed by the Damascene technique, which is one of the CMP techniques, thereby yielding the structure which has the interlayer contact hole 105 filled with the Cu film 109aand has the Ta film 106aexposed at the surface.
[0128] At this time, pure water to which Al2O3particles have been added is used as a polishing slurry, and the conditions such as the rotational polishing speed and applying load are varied depending on the material to be polished and the polishing amount.
[0129] Since the end of polishing is detected by a change in electric capacitance of the polished surface in the ordinary CMP technique, conventional methods have a difficulty in finely detecting the polishing end.
[0130] According to the second embodiment of this invention, however, because of the presence of the insulating film mask 108 under the Cu film 109a(see FIG. 6B), the electric capacitance temporarily increases when the Cu film 109ais polished to expose the insulating film mask 108, and the electric capacitance rapidly decreases when the insulating film mask 108 is completely polished. By detecting this change in electric capacitance, it is very easy to grasp the polishing stage of the Cu film 109aand detect the end of polishing.
[0131] According to the second embodiment, therefore, the polishing can be stopped the instant the Ta film 106ais exposed, preventing the Ta film 106afrom being removed. That is, this embodiment can effect polishing with higher controllability than the prior art methods.
[0132] Although a silicon dioxide film is used as the insulating film mask 108 in the second embodiment, this mask should not necessarily be a silicon dioxide film, but may be a silicon nitride film or a polyimide resin film which can provide an electric capacitance.
[0133] As shown in FIG. 6D, a Cu film 109bas the third conductive film is formed 250 to 500 nm thick by D.C. magnetron sputtering under the conditions of the pressure of 2 to 10 mTorr, the RF power of 1.0 to 5.0 KW, and the substrate temperature of 200 to 400° C., followed by the formation of a Ta film 106bas the fourth conductive film 20 to 50 nm thick on the top of the resultant structure.
[0134] The Cu film 109bas the third conductive film will serve as the main conductive film of the interconnection hat connects between semiconductor devices, and is formed of the same metal as the Cu film 109aused as the second conductive film in the second embodiment.
[0135] The Ta film 106bas the fourth conductive film is formed to (1) prevent Cu in a Cu film 109bas the third conductive film from being oxidized or corroded, (2) prevent reaction with the overlying insulating film and improve adhesion with that insulating film, and (3) improve the durability of the whole interconnection against electromigration and stress migration. In the first embodiment, the Ta film 106bis formed of the same metal used as the Ta film 106aas the first conductive film.
[0136] Next, an etching mask 110 made of a silicon nitride film is formed 200 to 400 nm thick on the Ta film 106aunder the conditions of 100 to 300 sccm of SiH4, 200 to 1200 sccm of NH3, the substrate temperature of 300 to 400° C., the pressure of 0.25 to 5.0 Torr and the RF power of 1.0 to 4.0 KW, and then the unnecessary portions are removed to yield the patterned interconnection by known lithography and dry etching techniques (see FIG. 6D).
[0137] Then, as shown in FIG. 6E, the Ta film 106b, the Cu film 109band the Ta film 106aare sequentially etched to pattern the interconnection by reactive ion etching using SiCl4, Cl2, NH3and N2under the conditions of the temperature of 280° C., the pressure of 2 Pa, 20 sccm of SiCl4, 20 sccm of Cl2, 10 to 30 sccm of NH3, 80 sccm of N2, and the RF power of 200 KW.
[0138] Further, the etching mask 110 and Ta film 106bon top of the Cu film 109band a reaction product whose composition is close to that of the silicon nitride film adhered to the side walls of the Ta film 106b, the Cu film 109band the Ta film 106aare removed by reactive ion etching using a fluorine gas such as CF4or CHF3.
[0139] The etching conditions should be selected in such a manner that the ratio of the etching speed of the silicon nitride film (etching mask 110) to the etching speed of the silicon dioxide film (insulating film 104a) is high and the silicon dioxide film (insulating film 104a) is hardly etched.
[0140] Then, a W film 111 having a thickness of 15 to 20 nm is selectively formed only around the interconnection (Cu film 109b) by the selective W-CVD technique using hydrogen as a reducing agent (FIG. 6E).
[0141] This selective growth of W is performed under the conditions: the temperature of 350 to 400° C., the pressure of 20 to 80 mTorr, 0.5 to 1.0 sccm of tungsten hexafluoride (WF6), and 200 to 400 sccm of H2. Under the conditions, depending on the ratio of the exposure of the metal film on the wafer, a slow W growth speed of about 5 to 7 nm/min is acquired, so that controlling the thickness of the W film is easy.
[0142] The W film 111 in the second embodiment is formed to protect the interconnection against corrosion and oxidation.
[0143] To obtain good selectivity in growing the W film 11, the following two pre-treatments should be performed.
[0144] First, a pretreatment with a thin hydrofluoric solution is performed to eliminate damage to the surface of the insulating film 104acaused during etching the Cu film 109band insulating film mask 108.
[0145] The other pretreatment uses a Cu-dissoluble solution such as thin sulfuric acid, and this treatment cleans the surface of the Cu film 109b.
[0146] Because the interlayer contact hole and the interconnection are connected by the same kind of metal in the semiconductor device according to the second embodiment fabricated by the above-described five step process, the contact resistance between the contact hole and the interconnection is lower than that of conventional semiconductor devices, thus ensuring excellent electric characteristics, as per the first embodiment.
[0147] Because the Ta film 106ahaving a high melting point is located above and under the interconnection and the W film covers the interconnection, the oxidation and corrosion of the Cu film as the main conductive film can be suppressed, thus allowing the interconnection to have high and continuing reliability.
[0148] Further, the groove-buried interconnection facilitates making the interconnection thicker, and it is easy to reduce its resistance.
[0149] The semiconductor device of the second embodiment, like that of the first embodiment, can be adapted for various kinds of semiconductor devices, such as MOS transistors and bipolar transistors, as well as various circuits like memory and logic.
Claims
Certificate of Correction present
The claims shown below may not include correction changes. Use the corrected PDF for authoritative text.
What is claimed is:
1. A semiconductor device having a metal interconnection, said metal interconnection including:
an insulating film provided on a semiconductor substrate via a diffusion layer;
an interlayer contact hole formed in said insulating film;
a metal silicide layer provided at a bottom of said interlayer contact hole;
a first conductive film, comprising at least one metal film, provided on said insulating film and said interlayer contact hole;
a second conductive film provided in said interlayer contact hole;
a third conductive film provided on said first conductive film and said second conductive film; and
a fourth conductive film provided on said third conductive film.
2. A semiconductor device having a metal interconnection, comprising:
an insulating film provided on a semiconductor substrate via a diffusion layer;
an interlayer contact hole formed in said insulating film;
a metal silicide layer provided at a bottom of said interlayer contact hole;
a first conductive film, comprising at least one metal film, provided on said insulating film and said interlayer contact hole;
a second conductive film provided in said interlayer contact hole;
a third conductive film provided on said first conductive film and said second conductive film; and
a fourth conductive film provided on said third conductive film.
3. The semiconductor device according to claim 1, wherein said first conductive film comprises at least one metal film of at least one type of material selected from the group consisting of titanium (Ti), zirconium (Zr), hafnium (Hf), vanadium (V), niobium (Nb), tantalum (Ta), chromium (Cr), molybdenum (Mo), tungsten (W), osmium (Os), cobalt (Co), iridium (Ir), nickel (Ni), palladium (Pd), platinum (Pt), and alloys and compounds containing those elements.
4. The semiconductor device according to claim 1, wherein said second conductive film and said third conductive film are formed of at least one type of material selected from the group consisting of aluminum (Al), copper (Cu), silver (Ag), gold (Au), and alloys containing those elements.
5. The semiconductor device according to claim 1, wherein said fourth conductive film is formed of at least one type of material selected from group consisting of titanium (Ti), zirconium (Zr), hafnium (Hf), vanadium (V), niobium (Nb), chromium (Cr), molybdenum (Mo), tungsten (W), and alloys and compounds containing those elements.
6. The semiconductor device according to claim 1, wherein said first conductive film and fourth conductive film are formed of the same material, and said second conductive film and third conductive film are formed of the same material.
7. The semiconductor device according to claim 2, wherein said first conductive film comprises at least one metal film of at least one type of material selected from the group consisting of titanium (Ti), zirconium (Zr), hafnium (Hf), vanadium (V), niobium (Nb), tantalum (Ta), chromium (Cr), molybdenum (Mo), tungsten (W), osmium (Os), cobalt (Co), iridium (Ir), nickel (Ni), palladium (Pd), platinum (Pt), and alloys and compounds containing those elements.
8. The semiconductor device according to claim 2, wherein said second conductive film and said third conductive film are formed of at least one type of material selected from the group consisting of aluminum (Al), copper (Cu), silver (Ag), gold (Au), and alloys containing those elements.
9. The semiconductor device according to claim 2, wherein said fourth conductive film is formed of at least one type of material selected from the group consisting of titanium (Ti), zirconium (Zr), hafnium (Hf), vanadium (V), niobium (Nb), chromium (Cr), molybdenum (Mo), tungsten (W), and alloys and compounds containing those elements.
10. The semiconductor device according to claim 2, wherein said first conductive film and fourth conductive film are formed of the same material, and said second conductive film and third conductive film are formed of the same material.
11. The semiconductor device according to claim 1, wherein said second conductive film is disposed substantially entirely within said interlayer contact hole, and said third and fourth conductive films are disposed substantially entirely outside said interlayer contact hole.
12. The semiconductor device according to claim 2, wherein said second conductive film is disposed substantially entirely within said interlayer contact hole, and said third and fourth conductive films are disposed substantially entirely outside said interlayer contact hole.
13. The semiconductor device according to claim 11, wherein said third conductive film has a top surface and a plurality of side surfaces, wherein said fourth conductive film is provided on said top surface of said third conductive film, and wherein said metal interconnection further comprises a fifth conductive film provided on said side surfaces of said third conductive film.
14. The semiconductor device according to claim 12, wherein said third conductive film has a top surface and a plurality of side surfaces, wherein said fourth conductive film is provided on said top surface of said third conductive film, and wherein said metal interconnection further comprises a fifth conductive film provided on said side surfaces of said third conductive film.
Patent Citations (7)
Non-Patent Literature (1)
- “Planar Copper-Polyimide Back End of the Line Interconnections for ULSI Devices,” B. Luther et al., 1993 Proceedings Tenth Internat'l. VLSI Multilevel Interconnection Conference, Santa Clara, CA, pp. 15-21, Jun. 8 and 9, 1993.Applicant