Background of the Invention
(1) Field of the Invention
The invention relates to the fabrication of integrated circuit devices, and more particularly, to a method of photoresist double coating to fabricate fine lines with narrower spacing than the resolution limit offered by the current best photolithography in the fabrication of integrated circuits.
(2) Description of the Prior Art
In the fabrication of integrated circuits, reductions in both the minimum line width and line spacing can lead to a denser circuit layout or smaller die size for the product. However, the minimum line width and line spacing on the wafer are limited conventionally by photolithography's resolution.
Referring to FIG. 1, there is shown a portion of a partially completed integrated circuit. A layer 12 which is to be etched is deposited over silicon substrate 10. Photoresist layer 14 coats the surface of the layer 12. As shown in FIG. 1, the photoresist layer 14 is patterned to create a photoresist mask. If the resolution of the photolithography process is R and the minimum misalignment tolerance between two layers is M, then the minimum pitch (line width (15)+line spacing (16)) is R+R=2R, by the conventional photolithographic process of the prior art.
U.S. Pat. No. 4,906,552 to Ngo et al describes a flood illumination patterning technique that achieves resolutions of 0.5 micrometers or less using a dual layer of photoresist. U.S. Pat. Nos. 5,091,290 to Rolfson, 4,704,347 to Vollenbroek et al, and 4,591,547 to Brownell all teach methods of dual layers of photoresist in which one layer of photoresist is at least partially over the other layer of photoresist.
Summary of the Invention
A principal object of the present invention is to provide an effective and very manufacturable method of providing narrow line spacing of less than the resolution limit of the photolithography process.
In accordance with the object of this invention a new photolithographic process using the method of photoresist double coating to fabricate fine lines with narrow spacing is achieved. A layer to be etched is provided overlying a semiconductor substrate. The layer to be etched is coated with a first layer of photoresist and baked. The first photoresist layer is exposed to actinic light through openings in a mask and developed to produce the desired first pattern on the surface of the first photoresist wherein the openings have a minimum width of the resolution limit plus two times the misalignment tolerance of the photolithography process. The layer to be etched is coated with a second photoresist layer where the layer to be etched is exposed within the openings in the first photoresist layer. The second photoresist layer is exposed to actinic light through openings in a mask and developed to produce the desired second pattern on the surface of the second photoresist wherein the second pattern alternates with the first photoresist pattern and wherein the spacing between the first and second patterned photoresist coatings has a width equal to the misalignment tolerance. The misalignment tolerance is much smaller than the resolution limit so the line spacing achieved is narrower than the resolution limit of the photolithography process.
Brief Description of the Drawings
In the accompanying drawings forming a material part of this description, there is shown:
FIG. 1 schematically illustrates in cross-sectional representation a photolithographic process of the prior art.
FIGS. 2 through 4 schematically illustrate in cross-sectional representation a preferred embodiment of the present invention.
FIGS. 5 through 8 schematically illustrate in cross-sectional representation additional embodiments of the present invention.
FIG. 9 schematically illustrates in cross-sectional representation a completed integrated circuit for one embodiment of the present invention.
Description of the Preferred Embodiments
Referring now more particularly to FIGS. 2 through 4, the photolithographic method of the present invention will be described. A layer 12 to be etched has been deposited over the surface of semiconductor substrate 10. This layer can be a single layer or multi-layers and can be a polysilicon word line or metal line or various other structures in the fabrication of an integrated circuit. Specific examples will be discussed in the Examples section to follow. The process of the invention is independent of the material to be etched.
A first layer of photoresist 14 is coated over the surface of the layer 12. A positive photoresist is used with a conventional thickness of between about 10,000 to 30,000 Angstroms. The photoresist layer 14 is exposed to actinic light through openings in a mask and developed to produce the desired pattern on the surface of the photoresist. The resulting resist mask layer 14 has openings of the size R+2M, where R is the line width and M is the misalignment tolerance.
The photoresist mask layer 14 is baked using an ultraviolet baking process at a temperature of between about 140.degree. to 160.degree. C. for between about 50 to 70 seconds. The ultraviolet baking process hardens the photoresist mask layer.
A second photoresist coating 18 is spun onto the wafer into the openings in the photoresist mask layer 14. The photoresist layer 18 is exposed to actinic light through openings in a mask 20, shown in FIG. 3, and developed to produce the desired pattern on the surface of the photoresist. Since the first photoresist mask 14 has been hardened by the ultraviolet baking process, it will not be removed during developing and etching of the second photoresist layer 18. The resulting resist mask layer is illustrated in FIG. 4. The spacing between the lines will be M instead of R as in the prior art. Since M is much smaller than R, the line spacing has been reduced dramatically by using the double photoresist coating method of the invention. For example, for the 0.6 micrometer design rule, R=0.6 micrometers and M is approximately=0.2 micrometers. After the layer 12 has been etched, the photoresist mask layer 14,18 can be stripped using a wet or dry photoresist stripping process, such as sulfuric acid or other stripper chemicals for a wet strip, or oxygen plasma for a dry strip.
Examples
The following Examples are given to show the important features of the invention and to aid in the understanding thereof and variations may be made by one skilled in the art without departing from the spirit and scope of the invention.
The following Examples will illustrate some applications for the double photoresist coating process of the invention. Referring now to FIG. 5, there is illustrated a buried bit mask read-only memory (ROM) process. The double photoresist mask 14 and 18 is fabricated as described above for FIGS. 2 through 4 on the surface of silicon substrate 10. An N+ ion implantation 19 into the substrate 10 through the openings in the photoresist mask forms buried bit lines 21. This process allows the designer to reduce the buried bit line openings and thus reduce the cell size of the memory.
Referring now to FIG. 6, there is illustrated another buried bit mask ROM process in which polysilicon word lines are to be fabricated. A gate silicon oxide layer 22 has been grown or deposited over the surface of the silicon substrate 10. A layer of polysilicon 24 is deposited over the surface of the silicon oxide. The photoresist mask 14 and 18 is fabricated using the double coating method of the invention. The mask will be used to etch polysilicon word lines, indicated by dotted lines within polysilicon layer 24. Reducing the space between the word lines will reduce the cell size of the memory. FIG. 9 illustrates the completed integrated circuit of this example showing the word lines 24 and passivation layer 30 of, for example, borophosphosilicate glass.
FIG. 7 illustrates a buried bit line or a NAND-typed double polysilicon erasable-programmable read-only memory (EPROM) or a Flash memory. A gate silicon oxide or tunnel silicon oxide layer 32 is grown or deposited on the surface of the silicon substrate 10. Layer 34 is a polysilicon floating gate layer. An interpoly dielectric layer 36 is deposited over the floating gate 34. This layer 36 is typically composed of a multiple ONO layer consisting of silicon oxide, silicon nitride, and silicon oxide. Finally, the control gate polysilicon layer 38 is deposited over the ONO layer. The double photoresist mask 14 and 18 is fabricated following the method of the present invention. A stacked gate composed of layers 38, 36, and 34 will be etched using the double photoresist mask of the invention as indicated by the dotted lines in FIG. 7. The double photoresist coating method increases the cell layout density of the memory.
FIG. 8 illustrates metal line definition. The semiconductor substrate 10, which may contain semiconductor device structures such as gate electrodes and source and drain regions, is covered with an insulating layer 42 composed of borophosphosilicate glass (BPSG), for example. A metal layer 44 is deposited over the BPSG layer. The double photoresist mask 14 and 18 of the invention is fabricated over the surface of the metal 44 and is used to etch metal lines as indicated by the dotted lines within layer 44 in FIG. 8.
The double photoresist coating method of the invention may be used in etching active isolation regions and in other etching applications in the manufacture of integrated circuits.
While the invention has been particularly shown and described with reference to the preferred embodiments thereof, it will be understood by those skilled in the art that various changes in form and details may be made without departing from the spirit and scope of the invention.