In the following some of the examples of the invention will be explained in detail by comparing with comparative examples. However, it is to be understood that the invention is not limited to the specific embodiments. In the explanations "part" means part by weight and "%" means % by weight. Physical properties of the polyetheresteramides and the resin compositions finally obtained were measured by the following testing methods.
Criteria of Evaluation
.circleincircle.:Good
.largecircle.:A little delamination observed
X :Numbers of delamination observed, Poor Compatibility
EXAMPLE 1
A blend of 105 parts .epsilon.-caprolactam, 17.1 parts adipic acid, 0.3 part Irganox 1010 (antioxidant manufactured by Ciba-Geigy, Ltd.) and 6 parts water was contained in a 3 liter stainless steel autoclave, which was then filled with nitrogen replacing air followed by heating at 220.degree. C. under pressure for 4 hours while stirring to obtain 117 parts polyamide oligomer with carboxyl chain ends having a number average molecular weight 1,000 and an acid value 110. The polyamide oligomer was then added with 225 parts ethylene oxide adduct of bisphenol A having a number average molecular weight 2,000 and 0.5 part Zirconium acetate, and the mixture was heated at 245.degree. C. to effect polymerization for 5 hours under reduced pressure lower than 1 mmHg to obtain a viscous polymer. The polymer was then taken out on a belt in the form of a strand, which was then pelletized to obtain the polyetherestermide of the invention. The relative viscosity of the polymer obtained was 2.15 as measured for a 0.5% by weight solution in m-cresol at 25.degree. C. The copolymer composition of the polymer as determined by NMR analysis was as follows.
The temperature of starting weight loss on heating of the polyetheresteramide obtained was measured by TG-DTA in nitrogen. Furthermore, using test pieces respectively prepared by injection molding, Izod impact strength according to ASTM D256, tensile strength according to ASTM D638 and surface resistivity by using a megohmmeter (made by Advantest Inc.), of the polyetheresteramide was measured. The surface resistivity was measured by using 2 mm thick square test pieces under the conditions of (a) not water washed, wherein square test pieces, after being molded, were held in an atmosphere of 20.degree. C. and 65% RH for 24 hours, and (b) water washed, wherein square test pieces, after being molded, were washed with an aqueous solution of a detergent (Mamalemon manufactured by Lion, Inc.) followed by washing with ionexchanged water and drying to remove surface moisture, and then held in an atmosphere of 20.degree. C. and 65% RH for 24 hours. The results of the measurements are tabulated in Table 1. The polyetheresteramide is hereafter named A-1.
EXAMPLE 2
A blend of 105 parts .epsilon.-caprolactam, 17.1 parts adipic acid, 0.3 part Irganox 1010 and 7 parts water was contained in a 3 liter stainless steel autoclave, which was then filled with nitrogen replacing air followed by heating at 220.degree. C. under pressure for 4 hours while stirring to obtain 117 parts polyamide oligomer with carboxyl chain ends having a number average molecular weight 1,100 and an acid value 100. The polyamide oligomer was then added with 225 parts ethylene oxide adduct of bisphenol A having a number average molecular weight 2,000 and 0.5 part Zirconium acetate, and the mixture was heated at 245.degree. C. to effect polymerization for 5 hours under reduced pressure lower than 1 mmHg to obtain a viscous polymer. The polymer was then processed in the same manner as described in Example 1 to obtain the polyetheresteramide of the invention. Physical properties of the polyetheresteramide were measured using the same methods as described in example 1. The results of the measurements are tabulated in Table 1. The polyetheresteramide is hereafter named A-2.
EXAMPLE 3
A composition of a polyetheresteramide and potassium chloride was obtained by the same method as described in Example 2 except that, when adding an ethylene oxide adduct of bisphenol A and Zirconium acetate, 2 parts potassium chloride was added together. The copolymer composition of the polyetheresteramide obtained as determined by NMR analysis was as follows.
The contents of the polyetheresteramide and potassium chloride as determined by X-ray fluorescence analysis was as follows.
Physical properties of the polyetheresteramide obtained were measured by the same methods as described in Example 1. The results of the measurements are tabulated in Table 1. The polyetheresteramide is hereafter named A-3.
EXAMPLE 4
A blend of 112 parts .epsilon.-caprolactam, 105 parts ethylene oxide adduct of bisphenol A having a number average molecular weight 1,000, 15 parts adipic acid, 0.3 part Irganox 1010, 0.5 part Zirconium acetate and 7 parts water was contained in a 3 liter stainless steel autoclave, which was then filled with nitrogen replacing air followed by heating at 220.degree. C. under pressure for 1.5 hours while stirring to obtain a homogeneous solution. It was confirmed that a polyamide oligomer having a number average molecular weight 1,250 and an acid value 90 was formed in the solution. Thereafter the solution was heated at 245.degree. C. to effect polymerization for 3.5 hours under reduced pressure to obtain a viscous polymer. The polymer was then processed in the same manner as described in Example 1 to obtain the polyetheresteramide of the invention. Physical properties of the polyetheresteramide were measured using the same methods as described in Example 1. The results of the measurements are tabulated in Table 1. The polyetheresteramide is hereafter named A-4.
EXAMPLE 5
A composition of a polyetheresteramide and sodium chloride was obtained by the same method as described in Example 4 except that, when adding an ethylene oxide adduct of bisphenol A and Zirconyl acetate, 3 parts sodium chloride was added together. The contents of the polyetheresteramide and sodium chloride as determined by X-ray fluorescence analysis was as follows.
Physical properties of the polyetheresteramide were measured using the same methods as described in Example 1. The results of the measurements are tabulated in Table 1. The polyetheresteramide is hereafter named A-5.
COMPARATIVE EXAMPLE 1
A polyetheresteramide for comparing with the polyetheresteramide of the invention was obtained by the same method as described in Example 1 except that 175 parts polyoxyethylene glycol having a molecular weight 1,500 was used instead of an ethylene oxide adduct of bisphenol A. Physical properties of the polyetheresteramide obtained were measured using the same methods as described in Example 1. The results of the measurements are tabulated in Table 1. The polyetheresteramide is hereafter named A-6.
COMPARATIVE EXAMPLE 2
A polyetheresteramide for comparing with the polyetheresteramide of the invention was obtained by the same method as described in Example 1 except that 175 parts polyoxyethylene glycol having a molecular weight 1,500 was used instead of an ethylene oxide adduct of bisphenol A and that polymerization was effected by heating for 3 hours. Physical properties of the polyetheresteramide were measured by the same methods as described in Example 1. The results of the measurements are tabulated in Table 1. The polyether-esteramide is hereafter called A-7.
COMPARATIVE EXAMPLE 3
A composition of a polyetheresteramide of Comparative example 1 and potassium chloride for comparing with the composition of the invention was obtained by the same method as described in Comparative Example 1 except that, when adding polyoxyethylene glycol and Zirconium acetate, 5 parts potassium choloride was added together. The contents of the polyetheresteramide and potassium choloride as determined by X-ray fluorescence analysis was as follows.
Physical properties of the polyetheresteramide obtained were measured by using the same methods as described in Example 1. The results of the measurements are tabulated in Table 1. The polyetheresteramide is hereafter named A-8.
In the following explanation the polymers A-1.about.A-8 will be called (A).
EXAMPLES 6 TO 9 AND COMPARATIVE EXAMPLES 4 TO 6
Each polyetheresteramide (A) obtained in the Examples and Comparative Examples described above was blended with each of the following resins B-1 to B-4 for 3 minutes using a Henschel mixer in a proportion shown in Table 2 for each Example. The blends obtained were melt kneaded using a vented double-screw extruder under a condition of 240.degree. C., 30 rpm and a residence time of 5 minutes to obtain the antistatic resin compositions of the invention and resin compositions for comparison.
B-1:ABS resin (JSR-ABS10 manufactured by Japan Synthetic Rubber, Inc.)
B-2:Nylon 6 resin (UBE Nylon 1013B manufactured by UBE Industries, Inc.)
B-3:Polybutylene terephthalate resin (Duranex 2000 manufactured by Polyplastics, Inc.)
B-4:Polypropylene resin (UBE Polypro J609 manufactured by UBE Industries, Inc.)
In the following explanations the above B-1 to B-4 are called (B) unless otherwise stated.
EXAMPLES 10, 11 AND COMPARATIVE EXAMPLE 7
The antistatic resin compositions of the invention and a comparative resin composition were obtained by the same process as described in Example 6 except that the melt kneading of (A) and (B) in the proportions shown in Table 2 was carried out at 250.degree. C.
EXAMPLES 12 TO 15 AND COMPARATIVE EXAMPLE 8
The antistatic resin compositions of the invention and a comparative resin composition were obtained by the same process as described in Example 6 by melt kneading (A) and (B) in the proportions shown in Table 2.
Performance Tests
Test pieces were prepared from the resin compositions of Examples 6 to 15 and Comparative Examples 4 to 8 using an injection molding machine under a condition shown in Table 3, which were tested for mechanical properties and antistatic property. The results of the measurements are tabulated in Tables 4 to 6. Tests for antistatic property were carried out by measuring the surface resistivity of the test pieces after having been treated and conditioned as described in Table 3.
Preparation of Compatibilizer
Preparation Example 1
A vinyl polymer containing sulfonic groups was obtained by the suspension polymerization of 68 parts methyl methacrylate, 23 parts styrene, 4 parts acrylonitrile and 5 parts of a compound containing sulfonic groups which is expressed by the following formula. The vinyl polymer containing sulfonic groups thus obtained is hereafter named C-1.
Structural Formula ##STR1##
Preparation Example 2
(1) A blend of 95 parts low-molecular weight polypropylene having a number average molecular weight 5,000 and a density 0.92 which was obtained by the thermal degradation of polypropylene and 5 parts maleic anhydride was melted at 180.degree. C. under nitrogen stream, followed by adding a 50% xylene solution in which 1.5 parts dicumyl peroxide are dissolved while dropping over 15 minutes. After the mixture was reacted for 1 hour, an acid modified low-molecular weight polypropylene was obtained by removing the solvent by distillation. The polymer obtained had an acid value of 25.4 and a molecular weight of 7,000.
(2) A styrene polymer containing hydroxyl groups was obtained by dissolving 95 parts styrene monomer in 100 parts xylene at 120.degree. C. under nitrogen, followed by adding 5 parts thioglycerine while dropping over 15 minutes, reacting for 1 hour and then removing the solvent and unreacted monomer by distillation. The polymer obtained had an hydroxyl value of 25.2 and a number average molecular weight of 8,000.
(3) A polypropylene-block-polystyrene needed was obtained by melt kneading 50 parts acid modified low-molecular weight polypropylene (1) and 50 parts styrene polymer containing hydroxyl groups (2) above-mentioned, by using a vented double-screw extruder under a condition of 200.degree. C., 30 rpm and a residence time of 5 minutes. The block polymer thus obtained is thereafter named C-2.
Preparation Example 3
A graft copolymer latex was obtained by the emulsion polymerization of 60 parts monomer mixture consisting of 4% by weight acrylic acid, 72% by weight styrene and 24 by weight acrylonitrile in the presence of 40 parts polybutadiene latex. The graft copolymer latex obtained was coagulated by sulfuric acid, neutralized by caustic soda, followed by washing, filtrating and drying to obtain a powdery reaction product of the graft copolymer (C-3).
Preparation Example 4
A mixture was obtained by melting a blend of 95 parts low-molecular weight polypropylene having a number average molecular weight 12,000 and a density 0.89 which was obtained by thermally degrading polypropylene and 5 parts maleic anhydride at 180.degree. C. under nitrogen stream, followed by adding a 50% xylene solution in which 1.5 parts dicumyl peroxide are dissolved while dropping over 15 minutes. After the obtained mixture was reacted for 1 hour, an acid-modified low-molecular weight polypropylene was obtained by removing the solvent by distillation. The polymer obtained had an acid value of 25.7 and a number average molecular weight of 15,000. The modified polymer thus obtained is hereafter named C-4.
Preparation Example 5
A modified low-molecular weight polypropylene containing hydroxyl groups was obtained by dissolving 95 parts acid-modified low-molecular weight polypropylene obtained in Preparation Example 4 (C-4) in 100 parts xylene at 120.degree. C. under nitrogen stream, followed by adding 5 parts monoethanolamine while dropping over 15 minutes, reacting for 1 hour and then removing the solvent and unreacted monoethanolamine by distillation. The polymer obtained had an hydroxyl value 25.2 and a molecular weight 16.000. The modified product thus obtained is hereafter named C-5.
Preparation Example 6
A polyoxyalkylene-modified low-molecular weight polypropylene was obtained by melting a blend of 95 parts acid-modified low-molecular weight polypropylene obtained in Preparation Example 4 (C-4) and 50 parts adduct of 24 mole ethylene oxide to lauryl alcohol at 180.degree. C. under nitrogen stream, followed by an esterification reaction for 5 hours under reduced pressure of 10 mmHg. The polymer obtained had an hydroxyl value of 0.5 and number average molecular weight of 18,000. By a NMR analysis, it was confirmed that the esterification reaction proceeded stoichiometrically. The modified product thus obtained is hereafter named C-6.
Preparation Example 7
An acid-modified low-molecular weight polyethylene was obtained by dissolving a mixture of 38 parts low-molecular weight polyethylene having a number average molecular weight 3,000 and a density 0.93 which was obtained by thermally degrading polyethylene and 2 parts maleic anhydride in 60 parts xylene at 140.degree. C. under nitrogen stream, followed by adding a 50% xylene solution in which 0.3 part di-t-butyl peroxide was dissolved while dropping over 15 minutes, reacting for 2 hours and removing the solvent by distillation. The polymer obtained had an acid value of 28.0 and a number average molecular weight of 3,800. The modified product thus obtained is hereafter named C-7.
In the following explanations the above compounds C-1 to C-7 will be called (C) unless otherwise stated.
Preparation of Master Batches 1
EXAMPLES 16 TO 19 AND COMPARATIVE EXAMPLES 9 TO 12
Polyetheresteramides (A), thermoplastic resins (B) and compatibilizers (C) were blended for 3 minutes in proportions shown in Table 7 for respective examples using a Henschel mixer. The blends obtained were melt kneaded using a vented double-screw extruder under a condition of 240.degree. C., 30 rpm and a residence time of 5 minutes to obtain respective master batches of Examples 16 to 19 and Comparative Examples 9 to 12, which will be called respectively M-1 to M-8 in the following according as they are described in Table 7.
EXAMPLES 20 TO 23 AND COMPARATIVE EXAMPLES 13 TO 16
The resin compositions of the invention and the compositions for comparison were obtained by blending and kneading masterbatches M-1 to M-8 and B-1 in the same manner as described in Example 16. The constitutions and the proportions of the resin compositions and the compositions for comparison prepared by way of the master batches are tabulated in Table 8.
COMPARATIVE EXAMPLES 17 TO 22
Polymers (A), (B) and (C) which are shown in Table 9 were blended and kneaded under the same condition as described in Example 16 to obtain respective resin compositions of the Comparative Examples.
Performance Tests
Test pieces were prepared by injection-molding the resin compositions of Examples 20 to 23 and Comparative Examples 13 to 21 and compositions for comparison at a cylinder temperature of 220.degree. C. and a mold temperature of 60.degree. C., which were tested for mechanical properties and antistatic property.
The results of the measurements are tabulated in Table 10. The tests for antistatic property were carried out by measuring the surface resistivity of the test pieces after having been treated and conditioned as described below.
Not water washed, wherein the test pieces, after having been molded, were held in an atmosphere of 20.degree. C. and 65% RH for 24 hours.
Water washed, wherein the test pieces, after having been molded, were washed with an aqueous solution of a detergent (Mamalemon manufactured by Lion, Inc.) followed by washing with ion-excahanged water and drying to remove surface moisture, and then held in an atmosphere of 20.degree. C. and 65% for 24 hours.
Preparation of Master Batches 2
EXAMPLES 24 AND 25
Polymers (A), (B) and (C) were blended in proportions shown in Table 11 for 3 minutes by using a Henschel mixer, followed by being melt kneaded by using a vented double-screw extruder under a condition of 280.degree. C., 100 rpm and a residence time of 5 minutes to obtain master batches M-9 and M-10 of Examples 24 and 25, respectively.
EXAMPLES 26 AND 27
The master batches M-9 and M-10 were respectively blended with B-5 under the same condition as described in Example 24 followed by kneading to obtain the resin compositions of the invention. The constitutions and proportions of the resin compositions of the invention by way of the master batches are tabulated in Table 12.
EXAMPLES 28 AND 29 AND COMPARATIVE EXAMPLES 23 AND 24
The polymers (A), (B) and (C) or (A), (B), (C) and (E) shown in Table 13 were blended respectively under the same condition as described in Example 24 followed by kneading to obtain the resin compositions of the invention and the resin compositions for comparison.
Performance Tests
Test pieces were prepared by injection-molding the resin compositions of examples 26 to 29, Comparative Examples 23 and and the resin compositions for comparison at a cylinder temperature of 270.degree. C. and a mold temperature of 70.degree. C., which were then tested for mechanical properties and antistatic property. The results of the measurements are tabulated in Table 14. The tests for antistatic property were carried out by measuring the surface resistivity of the test pieces after having been treated and conditioned as described below. Not water washed, wherein the test pieces, after having been molded, were held in an atmosphere of 20.degree. C. and 65% RH for 24 hours.
Water washed, wherein the test pieces, after having been molded, were washed with an aqueous solution of a detergent (Mamalemon manufactured by Lion, Inc.) followed by washing with ion-exchanged water and drying to remove surface moisture, and then held in an atmosphere of 20.degree. C. and 65% RH for 24 hours.
Preparation of Master Batches 3
EXAMPLES 30 TO 34 AND COMPARATIVE EXAMPLES 25 AND 26
The polymers (A), (B) and (C) were blended in proportions shown in Table 15 for 3 minutes by using a Henschel mixer, followed by being melt kneaded using a vented double-screw extruder under a condition of 240.degree. C., 30 rpm and a residence time of 5 minutes to obtain master batches M-11 to M-17 of Examples 30 to 34 and Comparative Examples 25 and 26, respectively.
EXAMPLES 35 TO 39 AND COMPARATIVE EXAMPLES 27 AND 28
The master batches M-11 to M-17 were respectively blended with B-2 and B-4, C-4 to C-6 and metal salts described in Table 16 followed by kneading under the same condition as described in Example 30 to obtain the resin compositions of the invention. The constitutions and proportions of the resin compositions of the invention by way of master batches are tabulated in Table 16.
EXAMPLES 40 to 45 and Comparative Examples 29 to 35
The polymers (A) to (C) described in Table 17, or (A) to (C) and metal salts described in Table 17 were blended and kneaded under the same condition as in Example 30 to obtain the resin compositions of the invention and the resin compositions for comparison.
Performance Tests
Test pieces were prepared by injection-molding the resin compositions of Examples 35 to 45, Comparative Examples 27 to 35 and the resin compositions for comparison at a cylinder temperature of 240.degree. C. and a mold temperature of 60.degree. C., which were then tested for mechanical properties and antistatic property. The results of the measurements are tabulated in Table 18. The tests for antistatic property were carried out by measuring the surface resistivity of the test pieces after having been treated and conditioned as described below.
Not water washed, wherein the test pieces, after having been molded, were held in an atmosphere of 20.degree. C. and 50% RH for 24 hours.
Water washed, wherein the test pieces, after having been molded, were washed with an aqueous solution of a detergent (Mamalemon manufactured by Lion, Inc.) followed by washing with ion-exchanged water and drying to remove surface moisture, and then held in an atmosphere of 20.degree. C. and 50% RH for 24 hours.
Preparation of Master Batches 4
EXAMPLES 46 AND 47 AND COMPARATIVE EXAMPLE 36
The polymers (A) to (C) were blended in proportions shown in Table 19 for 3 minutes by using a Henschel mixer, followed by being melt kneaded using a vented double-screw extruder under a condition of 240.degree. C., 100 rpm and a residence time of 5 minutes to obtain master batches M-18 to M-20 of Examples 46 and 47 and Comparative Examples 36, respectively.
EXAMPLES 48 TO 50 AND COMPARATIVE EXAMPLE 37
The master batches M-18 to M-20 were respectively blended with B-3, B-4 or B-7 shown in Table 19 followed by kneading under the same condition as described in Example 46 to obtain the resin compositions of the invention. The constitutions and proportions of the resin compositions of the invention by way of master batches are tabulated in Table 20.
EXAMPLES 51 TO 54 AND COMPARATIVE EXAMPLE 38
The polymers (A), (B) and (C) were blended in proportions shown in Table 21 followed by kneading under the same condition as described in Example 46 to obtain the resin compositions of the invention and the resin compositions for comparison.
Performance Tests
Test pieces were prepared by injection-molding the resin compositions of Examples 48 to 54, Comparative Examples 37 and 38 and the compositions for comparison at a cylinder temperature of 240.degree. C. and a mold temperature of 50.degree. C., which were then tested for mechanical properties and antistatic property. The results of the measurements are tabulated in Table 22. The tests for antistatic property were carried out by measuring the surface resistivity of the test pieces after having been treated and conditioned as described below.
Not water washed, wherein the test pieces, after having been molded, were held in an atmosphere of 20.degree. C. and 50% RH for 24 hours.
Water washed, wherein the test pieces, after having been molded, were washed with an aqueous solution of a detergent (Mamalemon manufactured by Lion, Inc.) followed by washing with ion-exchanged water and drying to remove surface moisture, and then held in an atmosphere of 20.degree. C. and 50% RH for 24 hours.