BACKGROUND
Syndiotactic polystyrene is a highly crystalline thermoplastic resin with a high melting point (in the 260.degree.-285.degree. C. range), a high crystallization rate, high chemical resistance and excellent mechanical properties which qualify it as thermoplastic engineering resin.
N. Ishihara et al, in a series of patents (Eur. Pat. Appl. EP 210,615, EP 275,943, Jpn. Kokai Tokkyo Koho JP 03 59,010) proposed a number of catalysts which can be employed for syndiospecific polymerization of styrene and its ring-substituted derivatives. All these catalysts include two components. The first component is a titanium compound, such as titanium tetraethoxide, cyclopentadienyltitanium trichloride, solid titanium-containing compounds derived from titanium tetrachloride, and tetrabenzyltitanium. The second component of their catalyst systems is methylaluminoxide which is produced by reacting trimethylaluminum (TMA) either with free water or with hydrates of inorganic salts, such as CuSO.sub.4.5H.sub.2 O. The said titanium compounds are inactive for styrene polymerization if, instead of methylaluminoxane, they are combined solely with trialkylaluminum compounds, such as TMA.
DETAILED DESCRIPTION
The invention relates to a combination of three components comprising a compound containing a transition metal belonging to the IVA Group of Periodic Table, TMA, and particular organotin compounds, can serve as syndiospecific catalysts for polymerization of styrene and its ring-substituted derivatives to highly syndiotactic polymers.
Thus, the catalyst components of this invention comprise:
(i) trimethylaluminum,
(ii) at least one of the organotin compounds with general formulae:
where R.sub.1, R.sub.2, R.sub.3, R.sub.4, R.sub.5 and R.sub.6 are the same or different C.sub.1 -C.sub.20 alkyl groups or aryl groups or alkylaryl groups.
(iii) one or several derivatives of transition metals having the formula Cp.sub.n MA.sub.m-n', wherein M is a metal belonging to the group of titanium, zirconium and hafnium; Cp is a cyclopentadienyl or a substituted cyclopentadienyl group wherein one or several substituents are alkyl groups of 1 to 6 carbon atoms; n is 0 or 1; m is 4 or 3. In preferred embodiments, n is 1, m is 4 and A belongs to the group consisting of a halogen, hydrogen, or an oxyhydrocarbyl group OR', wherein R' is a C.sub.1 -C.sub.6 linear or branched alkyl group, a substituted or non-substituted aryl group, or an arylalkyl group.
Typical examples of such transition metal compounds include tetraalkoxides of titanium, zirconium and hafnium, tetraphenoxides of titanium, zirconium and hafnium, monocyclopentadienyltitanium trihalides, monocyclopentadienyltitanium trialkoxides and monocyclopentadienyltitanium triphenoxides.
Typical examples of the employed organotin compounds include bis(triethyltin)oxide, bis(tri-n-butyltin)oxide, trimethyltin hydroxide, triethyltin hydroxide, tri-n-butyltin hydroxide, dimethyltin oxide, diethyltin oxide, di-n-butyltin oxide, methyltinhydroxide oxide, and n-butyltinhydroxide oxide. oxide, methyltinhydroxide oxide, and n-butyltinhydroxide oxide.
The only organoaluminum compound suitable for the use in these catalyst compositions is TMA. Other tested organoaluminum compounds, such as triethylaluminum, triisobutylaluminum, dimethylaluminum chloride, diethylaluminum chloride, ethylaluminum sesquichloride, and ethylaluminum dichloride were found unsuitable for the catalyst formation. An excess of TMA with respect to the organotin compound is required in order for these catalyst compositions to be active. The molar [TMA]:[organotin compound] ratio can be in the 1.05-1000 range, with the preferred range being 2 to 10.
The catalyst compositions comprising at least one of each of said three components polymerize styrene and substituted styrenes to homopolymers with the syndiotactic chain structure, and copolymerize styrene and various substituted styrenes. The substituted styrenes belong to the group of ring-substituted styrenes bearing one or several substituents chosen from an alkyl group, an alkylaryl group or a halogen.
The polymerization reactions can be carried out in slurry processes using pure styrenes or their mixtures with aromatic or aliphatic solvents, at temperatures ranging from 0.degree. to 150.degree. C.
The following examples demonstrate some of the principles of the invention and the nature of the catalyst components as well as the type of polymers produced with the catalyst compositions of the invention.
EXAMPLES
Example 1
To a glass bottle capped with a septum and flushed with nitrogen were added: 20 cc of purified toluene, 5 cc of purified styrene, 5.6 mmol of TMA (used as 20 wt.% solution in heptane), 1.4 cc (2.82 retool) of bis(tri-n-butyltin)oxide, [(n-C.sub.4 H.sub.9).sub.3 Sn].sub.2 O, and 0.0045 mmol of cyclopentadienyltitanium trichloride, C.sub.5 H.sub.5 TiCl.sub.3. The mixture was stirred by a magnet stirrer for 22 h at 25.degree. C. Then the content of the bottle was mixed with 5-time excess (by volume) of isopropanol and 1.33 g of crystalline syndiotactic polystyrene (yield 29.3% ) was recovered by filtration. The polymer had a melting point of 259.8.degree. C. 90.0% of the polymer was insoluble in methylethylketone.
Example 2
To a glass bottle capped with a septum and flushed with nitrogen were added: 20 cc of purified toluene, 5 cc of purified styrene, 7.0 mmol of TMA, 0.8 cc (1.61 mmol) of [(n-C.sub.4 H.sub.9).sub.3 Sn].sub.2 O, and 0.0045 mmol of C.sub.5 H.sub.5 TiCl.sub.3. The mixture was stirred by a magnet stirrer for 2 h at 60.degree. C. Then the content of the bottle was mixed with excess of isopropanol and 0.43 g of crystalline syndiotactic polystyrene (yield 9.4%) was recovered by filtration. The polymer had a melting point of 248.6.degree. C.
Example 3
To a glass bottle capped with a septum and flushed with nitrogen were added: 20 cc of purified toluene, 5 cc of purified styrene, 3.5 mmol of TMA, 0.30 g (1.66 mmol) of trimethyltin hydroxide, (CH.sub.3).sub.3 SnOH, and 0.0045 mmol of C.sub.5 H.sub.5 TiCl.sub.3. The mixture was stirred by a magnet stirrer for 24 h at 25.degree. C. Then the content of the bottle was mixed with excess of isopropanol and 0.32 g of crystalline syndiotactic polystyrene (yield 7.0%) was recovered by filtration.
Example 4
To a glass bottle capped with a septum and flushed with nitrogen were added: 20 cc of purified toluene, 5 cc of purified styrene, 3.8 mmol of TMA, 0.20 g (1.21 mmol) of dimethyltin oxide, (CH.sub.3).sub.2 SnO, and 0.0045 mmol of C.sub.5 H.sub.5 TiCl.sub.3. The mixture was stirred by a magnet stirrer for 22 h at 25.degree. C. Then the content of the bottle was mixed with excess of isopropanol and 0.53 g of crystalline syndiotactic polystyrene (yield 11.6%) was recovered by filtration.
Example 5
To a glass bottle capped with a septum and flushed with nitrogen were added: 20 cc of purified toluene, 5 cc of purified styrene, 5.6 mmol of TMA, 1.4 cc (2.82 retool) of [(n-C.sub.4 H.sub.9).sub.3 Sn].sub.2 O, and 0.0055 mmol of cyclopentadienyltitanium triphenoxide, C.sub.5 H.sub.5 Ti(OC.sub.6 H.sub.5).sub.3. The mixture was stirred by a magnet stirrer for 22 h at 25.degree. C. Then the content of the bottle was mixed with excess of isopropanol and 1.78 g of crystalline syndiotactic polystyrene (yield 39.2% ) was recovered by filtration. The polymer had a melting point of 250.3.degree. C. 89.7% of the polymer was insoluble in methylethylketone.
Example 6
To a glass bottle capped with a septum and flushed with nitrogen were added: 20 cc of purified toluene, 5 cc of purified styrene, 5.6 mmol of TMA, 1.4 cc (2.82 mmol) of [(n-C.sub.4 H.sub.9).sub.3 Sn].sub.2 O, and 0.0067 mmol of titanium tetraisopropoxide, Ti(Oi-C.sub.3 H.sub.7).sub.4. The mixture was stirred by a magnet stirrer for 22 h at 25.degree. C. Then the content of the bottle was mixed with excess of isopropanol and 0.83 g of crystalline syndiotactic polystyrene (yield 18.2% ) was recovered by filtration. The polymer had a melting point of 265.3.degree. C. 90.5% of the polymer was insoluble in methylethylketone.
Example 7
To a glass bottle capped with a septum and flushed with nitrogen were added: 50 cc of purified toluene, 20 cc of purified p-methylstyrene, 7.0 mmol of TMA, 2.0 cc (3.92 mmol) of [(n-C.sub.4 H.sub.9).sub.3 Sn].sub.2 O, and 0.0090 mmol of C.sub.5 H.sub.5 TiCl.sub.3. The mixture was stirred by a magnet stirrer for 20 h at 25.degree. C. Then the content of the bottle was mixed with excess of isopropanol and 5.77 g of amorphous poly(p-methylstyrene) (yield 32.1%) was recovered by filtration.
Example 8
To a glass bottle capped with a septum and flushed with nitrogen were added: 20 cc of purified toluene, 3.0 cc of purified styrene, 2.0 cc of purified p-methylstyrene, 2.8 mmol of TMA, 0.7 cc (1.412 mmol) of [(n-C.sub.4 H.sub.9).sub.3 Sn].sub.2 O, and 0.0045 mmol of C.sub.5 H.sub.5 TiCl.sub.3. The mixture was stirred by a magnet stirrer for 22 h at 25.degree. C. Then the content of the bottle was mixed with excess of isopropanol and 0.66 g of amorphous styrene-p-methylstyrene copolymer (yield ca. 14%) was recovered by filtration. The copolymer had a softening point of 122.degree. C.