US 5,198,512 AGrant
Polymerization Catalyst and Process
Issue Date:1993-03-30
•20 Claims
Abstract
A composition of matter is provided comprising a catalytic mixture resulting from contacting at least one of each of the following compounds, an pyridine compound, a clay compound, and an organo-nickel compound. Additionally, a process is provided comprising contacting, under polymerization conditions, at least one alpha-olefin, wih a catalytic mixture resulting from contacting at least one of each of the following compounds, an pyridine compound, a clay compound, and an organo-nickel compound.
Metadata
Assignee
- Phillips Petroleum Company
Inventors
- Margie F. Jackson
- Ronald D. Knudsen
- Joseph S. Shveima
Application Information
Application Number:US 808128&
Filing Date:1991-12-16
Priority Date:1991-12-16
Art Unit:116
Classifications
IPC:
C08F 480
Field of Search:
526130;147
Patent Drawings
This patent does not have any drawings.
Description
Background of the Invention
This invention relates to the field of alpha-olefin polimerization.
Various polymerization processes are known in the art. For example, both chromium and titanium catalyst systems are known to polymerize ethylene. However, even these two popular polymerization systems do not provide solutions to all consumer demands. Consequently, research has been conducted to find new and better polymerization schemes.
One of the important polymer properties is the molecular weight of the polymer. For example, the molecular weight of polyethylene can influence the following properties of the resin: tensile strength; tear strength; low temperature toughness; softening temperature; impact strength; environmental stress crack resistance; melt fluidity; and melt drawability. Consequently, methods are constantly sought which would provide a means to control the molecular weight of a polyolefin.
Summary of the Invention
It is an object of this invention to provide an improved polymerization process.
It is another object of this invention to provide an improved polymerization process which provides an improved molecular weight control.
It is still another object of this invention to provide an improved catalyst system.
It is still yet another object of this invention to provide an improved catalyst system which provides improved molecular weight control.
In accordance with this invention a composition of matter is provided comprising a catalytic mixture resulting from contacting at least one of each of the following compounds, an pyridine compound, a clay compound, and an organo-nickel compound.
In another embodiment of this invention a process is provided comprising contacting, under polymerization conditions, at least one alpha-olefin, with a catalytic mixture resulting from contacting at least one of each of the following compounds, an pyridine compound, a clay compound, and an organo-nickel.
Detailed Descriptions of the Invention
Pyridine Compounds
The pyridine compounds useful in this invention are those compounds which are characterized by the following formula: ##STR1## wherein each R is independently selected from the group consisting of Hydrogen and --COOH, provided that at least one R is a --COOH group. Examples of suitable compounds include, but are not limited to, pyridine-2-carboxylic acid (also known as picolinic acid), pyridine-3-carboxylic acid (also known as nicotinic acid), pyridine-4-carboxylic acid, pyridine-2,4-dicarboxylic acid, pyridine-2,5-dicarboxylic acid and pyridine-2,4,6-tricarboxylic acid. Preferred compounds are the mono-pyridine carboxylic acids and most preferred is pyridine-2-carboxylic acid.
The molar ratio of acid compound to nickel should initially be in the range of about 0.01 to about 2. Preferably the molar ratio of acid compound to nickel is in the range of about 0.25 to about 1.75 and most preferably it is in the range of 0.5 to 1.5 inclusive. These ranges during the initially contacting of the catalyst reactants are important because of the resulting complex reactions after contacting.
Clay Compounds
Various clays can help form a polymer of high molecular weight. The initial weight ratio of the clay compound to nickel is generally in the range of about 1 to about 500. Preferably the weight ratio of clay compound to nickel is in the range of about 10 to about 300 and most preferably it is in the range of 25 to 200 inclusive. These ranges during the initial contacting of the catalyst reactants are important because of the resulting complex reactions after contacting and because of various economic and polymer considerations.
General classes of clay compounds useful in this invention are aluminum silicates, magnesium silicates, or aluminum-magnesium silicates. Examples of suitable clay compounds useful in this invention include, but are not limited to:
(1) attapulgite, an aluminum-magnesium silicate.
(2) bentonite, an aluminum silicate.
(3) halloysite, an aluminum silicate.
(4) hectorite, a magnesium silicate.
(5) kaolinite, an aluminum silicate.
(6) montmorillonite, an aluminum silicate.
(7) pyrophylite, an aluminum silicate.
(8) sepiolite, a magnesium silicate.
(9) talc, a magnesium silicate.
(10) vermiculite, an aluminum-magnesium silicate.
Particularly preferred clay catalyst supports are the magnesium silicates such as sepiolite.
It is preferred that the clay compound be conditioned prior to use. This conditioning comprises subjecting the clay compound to a conditioning temperature in the range of about 200.degree. to about 800.degree. C., preferably about 300.degree. to about 700.degree. C., and most preferably 400.degree. to 600.degree. C. The clay compound should be subjected to this conditioning temperature for a period of about 5 minutes to about 50 hours, preferably about 30 minutes to about 25 hours, and most preferably 1 hour to 10 hours.
Organo-Nickel Compounds
The characteristics of these compounds are as follows. The nickel component of the comound should already be in a zero valence state or it should be able to undergo reduction to a zero valence state, before formation of the active nickel component. The organic component should be an unsaturated, compound. An example of a nickel compound useful in this invention is bis(1,5-cyclooctadiene) nickel (referred to hereafter as (COD).sub.2 Ni).
These three components of the catalytic mixture, (pyridine compound, clay compound, and organo-nickel compound), can be contacted in any order and in any manner known in the art.
Alpha-olefins
The alpha-olefins which can be polymerized by this invention are those alpha-olefins with 2 to about 16 carbon atoms in the molecule. Preferably the alpha-olefin molecules have from 2 to about 12 carbon atoms and most preferably they have 2 to 8 carbon atoms. Furthermore, these alpha-olefins can either be linear or branched. Examples of alpha-olefins suitable for this invention include, but are not limited to, ethylene, propylene, 1-butene, 3-methyl-1-butene, 1-pentene, 3-methyl-1-pentene, 4-methyl-1-pentene, 1-hexene, 3-ethyl-1-hexene, 1-octene, 1-decene. It is also within the scope of this invention to copolymerize any of the above monomers with one of the other monomers.
Polymerization Conditions
The reaction temperature can be in the range of about 0.degree. C. to about 300.degree. C. Preferably the reaction temperature is between about 10.degree. C. and about 200.degree. C. and most preferably it is in the range of 20.degree. C. to 160.degree. C. inclusive. The reaction pressure can be in the range of about 10 psig to about 10000 psig. Preferably it is in the range of about 50 to about 1000 psig and most preferably it is in the range of 100 to 600 psig. The reaction time can be in the range of about 1 minute to about 100 hours. Preferably it is in the range of about 5 minutes to about 50 hours and most preferably it is in the range of 1 to 10 hours.
Examples
These examples are provided to further assist a person skilled in the art with understanding this invention. The particular reactants, conditions, and the like, are intended to be generally illustrative of this invention and are not meant to be construed as unduly limiting the reasonable scope of this invention.
In each run below, ethylene was contacted with (COD).sub.2 Ni, picolinic acid, if used, and either bentonite or sepiolite, if used. The reactions were conducted in a 1 liter, stainless steel, stirred reactor. The reactor's contents were substantially free from oxygen which would have adversely affected the polymerization reaction.
A solvent and either the bentonite or the sepiolite, if used, were added to the reactor first. These components were then briefly stirred after being purged with ethylene. Subsequent to this stirring the (COD).sub.2 Ni, and the picolinic acid, if used, were added to the reactor. The chemicals in the reactor were then stirred for about 15 minutes. Ethylene was then pressured into the reactor along with a comonomer, if used. The ethylene pressure was then maintained at a nearly constant pressure. The reactions were then terminated by venting the excess ethylene. Any resulting solid material was then separated and recovered. In general, the recovered solid was washed in toluene and/or methanol and then dried and weighed. Thereafter, the characteristics of the solid material were determined.
The results are presented in Tables I-A, I-B, I-C, I-D and I-E. The run numbers in each table refer to the same run (i.e. run 1 in Table I-A, is also run 1 in Table I-B).
As can be seen from the above, the pyridine compound is very important to the polymerization. This is evidenced by run number one which discloses that without the pyridine compound no polymer was formed. Furthermore, the importance of the clay compound is evidenced by run numbers thirteen and fourteen. In these runs it is evident that without the clay compound very low productivities were obtained. It should be noted that run number ten is considered an abnormal run that is not consistent with this invention.
The data in Table I-E discloses that very low melt indexes are achieved with the clay compounds. This is evidenced by runs 2, 3, 5-9, and 11 when compared to runs 13 & 14.
Claims
That which is claimed is:
1. A process comprising contacting, under polymerization conditions, at least one alpha-olefin, with a catalytic mixture resulting from contacting at least one pyridine compound having the formula ##STR3## wherein each R is independently selected from the group consisting of hydrogen and --COOH, provided that at least one R group is a --COOH group, at least one organo-nickel compound wherein the nickel is in the zero valence state or said nickel is able to undergo reduction the zero valence state before formation of the active nickel component, and at least one clay compound wherein the weight ratio of said clay compound to said nickel is from about 1 to about 500.
2. A process according to claim 1 wherein said polymerization conditions comprise a reaction temperature of about 0.degree. C. to about 300.degree. C., a reaction pressure of about 10 psig to about 10000 psig, and a reaction time of about 1 minute to about 100 hours.
3. A process according to claim 1 wherein said alpha-olefin has 2 to about 12 carbon atoms per molecule.
4. A process according to claim 1 wherein said alpha-olefin is selected from the group consisting of ethylene, propylene, 1-butene, 3-methyl-1-butene, 1-pentene, 3-methyl-1-pentene, 4-methyl-1-pentene, 1-hexene, 3-ethyl-1-hexene, 1-octene, 1-decene, and mixtures thereof.
5. A process according to claim 1 wherein said alpha-olefin is ethylene.
6. A process according to claim 1 wherein said pyridine compound is selected from the group consisting of pyridine-2-carboxylic acid, pyridine-3-carboxylic acid, pyridine-4-carboxylic acid, pyridine-2,4-dicarboxylic acid, pyridine-2,5-dicarboxylic acid, pyridine-2,4,6-tricarboxylic acid, and mixtures thereof.
7. A process according to claim 1 wherein said pyridine compound is selected from the group consisting of pyridine-2-carboxylic acid, pyridine-3-carboxylic acid, pyridine-4-carboxylic acid, and mixtures thereof.
8. A process according to claim 1 wherein said pyridine compound is pyridine-2-carboxylic acid.
9. A process according to claim 1 wherein the molar ratio of pyridine compound to nickel is from about 0.01 to about 2.
10. A process according to claim 1 wherein said clay compound is selected from the group consisting of aluminum silicate clays, magnesium silicate clays, aluminum-magnesium silicate clays, and mixtures thereof.
11. A process according to claim 1 wherein said clay compound is selected from the group consisting of attapulgite, bentonite, halloysite, hectorite, kaolinite, montmorillonite, pyrophylite, sepiolite, talc, vermiculite, and mixtures thereof.
12. A process according to claim 1 wherein said clay compound is a magnesium silicate clay.
13. A process according to claim 1 wherein said clay compound is selected from the group consisting of sepiolite, bentonite, and mixtures thereof.
14. A process according to claim 1 wherein said clay compound is sepiolite.
15. A process according to claim 1 wherein said clay compound is bentonite.
16. A process according to claim 1 wherein the weight ratio of clay compound to nickel is from about 1 to about 500.
17. A process according to claim 1 wherein said nickel compound is bis(1,5-cyclooctadiene) nickel.
18. A process comprising contacting: (a) under polymerization conditions comprising, a reaction temperature of about 0.degree. C. to about 300.degree. C., a reaction pressure of about 10 psig to about 10000 psig, and a reaction time of about 1 minute to about 100 hours; (b) ethylene; with (c) a catalytic mixture resulting from contacting (1) pyridine-2-carboxylic acid; (2) bis(1,5-cyclooctadiene)nickel; and (3) a clay compound selected from the group consisting of sepiolite, bentonite, and mixtures thereof, wherein the weight ratio of clay compound to nickel is from about 1 to about 500.
19. A process according to claim 18 wherein the molar ratio of pyridine-2-carboxylic acid to nickel is from about 0.01 to about 2.
20. A process according to claim 18 wherein the weight ratio of clay compound to nickel is from about 10 to about 300.