PRODUCTION EXAMPLE 1
Production of aqueous polyurethane resin (A),
1,780 g of 1,6-hexanediol, 2,545 g of adipic acid and 567 g of 2,2-dimethylolpropionic acid were mixed, heated to 170.degree. C, and reacted for 23 hours at that temperature to obtain a polyester polyol having a hydroxyl value of 60 and an acid value of 60.
The polyester polyol was diluted with 1,815 g of methyl ethyl ketone To 240 g of the resulting polyester polyol solution (I) were added 220 g of methyl ethyl ketone, 30 g of 2,2-dimethylolpropionic acid and 27 g of cyclohexanedimethanol, and they were stirred. To the mixture was added 236 g of 4,4'-dicyclohexylmethane diisocyanate. They were heated to 80.degree. C., reacted for 6 hours, and cooled to 30.degree. C. to obtain an urethane prepolymer solution.
The urethane prepolymer was slowly poured into an aqueous amine solution obtained by dissolving 21 g of an 80% aqueous hydrazine solution and 40 g of triethylamine in 1,500 g of deionized water, with stirring at a high speed, to obtain a viscous translucent product. The product was heated at 55.degree. C under reduced pressure to remove the solvent. Thereto was added deionized water to effect concentration adjustment to obtain a translucent aqueous polyurethane resin (A-1) having a non-volatile content of 23.7%, a viscosity (BM viscometer, 60 rpm, 25.degree. C.) of 23 cps and a pH of 8.4.
An aqueous polyurethane resin (A-2 to A-4) having the properties shown in Table 1 was prepared in the same manner as above, using the materials shown in Table 1.
PRODUCTION EXAMPLE 2
Production of aqueous dispersion B of acrylic copolymer
The following materials were prepared.
Aqueous dispersions (B-2) to (B-4) of acrylic copolymers having the properties shown in Table 2 were prepared in the same manner as above, using the materials shown in Table 2.
The aqueous polyurethane resins (A-1) and (A-4) obtained in Production Example 1 and the aqueous dispersions (B-1) to (B-4) of acrylic copolymers obtained in Production Example 2 were compounded as in Table 3-1 to prepare aqueous coating compositions of Examples 1-6 and Comparative Examples 1-9.
The following materials were prepared.
To a four-necked flask were fed 30 g of the above surfactant, 210 g of the above deionized water and 1.054 g of an aqueous polyurethane resin (A-1), and stirring was initiated. The mixture was heated to 80 .degree. C. in a nitrogen stream and the above polymerization initiator was added. Separately, 500 g of the above radicalpolymerizable monomers, 20 g of the above surfactant and 150 g of the above deionized water were mixed to prepare a monomer preemulsion. This monomer preemulsion was dropped into the above flask in 3 hours. The reaction temperature was maintained at 80.+-.3.degree. C.
After the completion of the dropping, the reaction was continued for a further 2 hours with stirring while maintaining the same temperature. The reaction mixture was cooled and adjusted to pH 8-9 with a 14% ammonia water to obtain an aqueous coating composition of Example 7 having a non-volatile content of 38.0%, a viscosity of 200 cPs and pH 8.5.
Aqueous coating compositions of Examples 8-11 and Comparative Examples 10-14 were obtained in the same manner as in Example 7, using the materials shown in Table 3-2.
The results of Examples 7-11 and Comparative Examples 10-14 are shown in Table 3-2.
COMPARATIVE EXAMPLE 15
Emulsion polymerization was conducted in the same manner as in Example 7 except that the aqueous polyurethane resin (A-1) was not used, to obtain an acrylic copolymer emulsion.
The emulsion had a non-volatile content of 55.1%, a viscosity of 3.300 cPs and pH 8.5
COMPARATIVE EXAMPLE 16
The aqueous polyurethane resin (A-1) per se was used in this Comparative Example to examine the effect of its combination use with an acrylic polymer.
The aqueous coating compositions of Examples 7-11 and Comparative Examples 10-16 were tested for properties when made into a film by itself using no additive. The results are shown in Table 4.
Test methods
(1) Water resistance
A sample was coated on a glass plate by a 3-mil applicator and dried for 3 days at room temperature. The resulting coating film was immersed in water for 7 days at room temperature and then the film condition was examined visually. (.largecircle. indicates a good film condition; .DELTA. indicates a normal film condition; and X indicates a poor film condition. These rating criteria also apply hereinafter.)
(2) Alkaline resistance
The coating film prepared in the same manner as in (1) above was immersed in a 2% aqueous NaOH solution for 7 days and then the film condition was examined visually.
(3) Solvent resistance
The coating film prepared in the same manner as in (1) above was immersed in methyl ethyl ketone for 1 day and then the film condition was examined visually.
(4) Abrasion resistance
A sample was coated on a standard tile (a vinyl-asbestos tile) for testing according to the JFPA specification, in an amount of 10.+-.2 ml per m.sup.2 of said tile. Coating was effected 5 times in the same manner. The resulting test piece was dried for 7 days at normal temperature and tested for extent of abrasion using a Taber machine (abrasion ring: CS-17, load: 1,000 g).
(5) Stress and strain of coating film
A sample was coated on a glass plate so that the resulting film had a thickness of 0.2 mm after drying, and then dried for 7 days.
(6) Flow-starting temperature
A sample was coated on a glass plate and dried for 7 days. 1.5-2.0 g of the resulting coating film was used and measured for flow-starting temperature (by using Koka flow Tester) under conditions of a temperature elevation speed of 3.degree. C./min, a load of 30 kgf and a die of 1 mm.phi..times.1 mml.
Test results
As is clear from Table 4, the aqueous coating compositions, as compared with other compositions not meeting the requirements of the present invention, are very superior in abrasion resistance, solvent resistance and stress and strain of coating film. Further, they have a far higher flow-starting temperature. Therefore, it is understood that the aqueous coating compositions of the present invention have a functional bond between aqueous urethane resin and acrylic resin.
Using the aqueous coating compositions obtained according to the compounding recipes shown in Table 3-2, elastic coating were prepared according to the following compounding recipes.
The above materials were dispersed by a high speed disperser. Then, the following materials were added thereto.
Using the above compounding recipes, the aqueous coating compositions of Examples 7-11 and Comparative Examples 10-16 were made into respective coating films and the films were measured for properties. The results are shown in Table 5.
Test method
Viscosity of coating:
A coating was measured for viscosity (cPs) by a BH type viscometer (4 rpm). Gloss of coating film:
A coating was coated on a glass plate by a 3-mil applicator and dried for 1 day. The resulting film was measured for reflectance (%) of 60.degree. /60.degree. .
Strain (JIS A 6910):
A sample was prepared so that the coating film had a thickness of about 1 mm when dried. It was aged according to the JIS method for strain and subjected to punching by No. 2 dumbbell. The resulting piece was used as a test piece. (Coating.fwdarw.aging for 7 days.fwdarw.back side aging for 7 days.fwdarw.punching)
Deterioration when extended (JIS A 6910):
The above sample piece was subjected to punching by No. 1 dumbbell. The resulting piece was used as a test piece.
Strength of adhesion (JIS A 6910):
Acrydic 53-448 was coated as a primer and dried for 3 hours. Then, a sample was coated thereon according to the test method and aged for 14 days. The resulting material was used for testing. Incidentally, the test material used for adhesion strength after immersion in water had been coated at the four sides with a vinyl chloride resin coating, 3 days befoe the completion of the aging. The adhesive used was a two-pack type epoxy adhesive.
Resistance to repeated hot-cold cycles:
A cycle consisting of (18 hours in water of 20.+-.2.degree. C. .fwdarw.3 hours at -20.+-.3.degree. C. .fwdarw.3 hours at .+-.50.+-.3.degree. C.) was repeated 10 times (total 10 cycles).
Water permeability:
Measured according to the JIS test method for extensive types.
Impact resistance:
Measured according to the JIS test method for extensive types.
Weather resistance:
Measured according to the JIS test method for extensive types.
Stress of coating film:
The stress of coating film when strain by JIS A 6910 was measured, was recorded.
Accelerated weather resistance:
The same coating film as used in the measurement of strain was subjected to light exposure for 50 hours in a standard weatherometer and then measured for strain at 20.degree. C. and -10.degree. C.
Test results
As is clear from Table 5, the aqueous coating compositions of the present invention, also when compounded with a pigment, have good weather resistance and the strengths of the resulting coating films do not deteriorate even after immersion in water.
The aqueous coating compositions of Examples 1-6 and Comparative Examples 1-9 were made into films by themselves using no additive, and the films were measured for properties. The results ar shown in Table 6-1.
Test results
As is clear from Table 6-1, the aqueous coating compositions of the present invention, even when no pigment is compounded, have good weather resistance, and the strengths of the resulting coating films do not deteriorate even after immersion in water.
Using the aqueous coating compositions of Examples 1-6 and Comparative Examples 1-9, elastic coatings were prepared according to said compounding recipes. The respective coating films were measured for properties. The results are shown in Table 6-2.
Test results
As is clear from Table 6-2, the aqueous coating compositions of the present invention, also when compounded with a pigment, have good weather resistance and the strengths of the resulting coating films do not deteriorate even after immersion in water.