US 5,141,814 AGrant
Addition Polymer Particles
Issue Date:1992-08-25
•25 Claims
Abstract
Very small (100 nanometers maximum) non-ionically-stabilized core-sheath addition polymer particles, wherein the core is addition polymer and the sheath polyoxylkylene chains, at least a portion of which chains are bonded to the core, there being present on each core sufficient chains such that the mass ratio of core to sheath is from 98:2 to 60:40. The particles are prepared by polymerization in aqueous media initiated at under 40.degree. C. In a preferred embodiment, a seed-feed process is used. The dispersions exhibit excellent rheological characteristics and are useful, for example, as film-formers in coating compositions.
Metadata
Assignee
- ICI Australia Operations Proprietary Ltd.
Inventors
- Geoffrey B. Anderson
- David S. Bignell
- Iain B. Cook
- Bruce Leary
- Christopher J. Lyons
Application Information
Application Number:US 4978498
Filing Date:1990-03-23
Priority Date:1989-03-23
Art Unit:159
Classifications
IPC:
B32B 2704
Field of Search:
428524402;407;516;519558;458;512;459
Patent Drawings
This patent does not have any drawings.
Description
Example 1
Preparation of particles of about 50 nm diameter, having a formulated core: sheath mass ratio of 88:12, the polyoxyalkylene chains having on average about 10 oxyethylene units. The process is a single stage process.
The following components were weighed into a reaction vessel:
("Ocenol" 110-130 (ex Henkel KGaA) is a commercially-available blend of C.sub.18 straight chain unsaturated alcohols having on average about 1.6 ethylenic double bonds per molecule. "Ocenol" is a trade mark).
The mixture was stirred and 30% w/w hydrochloric acid was added until a pH of less than 4 was achieved (0.2 parts was required). The mixture was cooled by means of an ice bath to less than 6.degree. C. and 4.13 parts of a 10% w/w aqueous solution of sodium erythorbate and then 0.75 parts of a 1% w/w aqueous solution of ferrous sulphate heptahydrate were added. Stirring was maintained as was external cooling to keep the exotherm temperature from exceeding 35.degree. C. The peak temperature was reached at about 15 minutes after the erythorbate/ferrous sulphate addition and stirring was continued for a further two hours.
The product was a translucent dispersion with a weight solids content of 50%. Examination by electron microscopy revealed particles of fairly uniform particle diameter of about 50 nm. Particle size measurements taken in a "Nanosizer" (trade mark) particle size measurement apparatus gave a diameter of 57 nm with a polydispersity of 4.
The proportion of polyoxyalkylene chains reacted on to the particles was determined to be 25% by GPC analysis of peak height at the retention time of the unreacted (not covalently bonded) chains.
The rheology and solids content of the dispersion rendered it ideal for use in a coating composition--it was found that none of the conventional rheology modifiers were needed. Viscosities were found to be as follows:
Viscosity (ICI cone and plate viscometer) at 10,000 s.sup.-1 1.1 poise
Viscosity (Haake RV100 viscometer) in the range 10-100 s.sup.-1 10 poise
This shows that the dispersion had rheological characteristics which were close to Newtonian in the low to medium shear rate range. In a paint which utilised the dispersion as a film-former, this gave very favourable brush pick-up, in-can appearance and excellent flow out, leading to the absence or near absence of brush marks in final film. The dispersion shear-thinned to about 1 poise at high shear rates (typical of those encountered during paint brushing), and this endowed the paint with excellent brushing properties.
Paint compositions formulated using the dispersion as film-former exhibited these excellent properties without the need to use added rheology-modifying agents. This additionally had the effect of keeping high the solids content and ensuring good film build on application.
Example 2
Preparation of particles of about 45 nm diameter, having a formulated core:sheath mass ratio of 90:10, the polyoxyalkylene chains having an average about 10 oxyethylene units. The process is a seed-feed process wherein no polymerisation is initiated until the feed has begun (hereinafter referred to as "Type A").
The following materials and proportions were used:
The seed stage materials were mixed, stirred and adjusted in pH to 4 with 30% w/w hydrochloric acid. The mixture was then cooled to 7.degree. C. and the feed stage was added over a period of 1 hour. During this period, the mixture exothermed but the temperature was kept below 30.degree. C. by means of external cooling.
The product was a translucent dispersion of polymer. The weight solids of the dispersion was 51% and, the particle diameter was 45 nm as measured by small angle x-ray scattering (SAXS) and 65 nm, polydispersity 5, as measured by "Nanosizer"apparatus.
Example 3
Preparation of particles of about 50 nm diameter, having a formulated core:sheath mass ratio of 89:11, the polyoxyalkylene chains having on average about 9.3 oxyethylene units. This example was a Type A seed-feed process (see Example 2) and ethoxylated methacrylic acid provided part of the sheath.
Example 2 was repeated, except that the ethoxylated "Ocenol" 110-130 was replaced by the following materials:
and that the mixture was maintained at below 30.degree. C.
The product was a translucent dispersion of polymer particles. The weight solids of the dispersion was 51% and particle diameter was 50 nm by SAXS and 85 nm with a polydispersity of 3 by "Nanosizer" apparatus.
Example 4
Preparation of particles of about 43 nm diameter, having a formulated core:sheath mass ratio of 88:12. the polyoxyalkylene chains having on average about 13 oxyethylene units. This example was a Type A seed-feed process (see Example 2) and derived its covalently bound sheath entirely from ethoxylated methacrylic acid.
Example 3 was repeated except that the ethoxylated "Ocenol" 110-130 was replaced by the same quantities in the stages of a nonylphenol-15 ethylene oxide surfactant (the actual surfactant used was "Teric" (Trade Mark) N15 ex ICI Australia Limited).
The product was a translucent dispersion of polymer particles. The dispersion weight solids was 51% and the particle diameter was 43 nm (by electron microscopy) and 52 nm, polydispersity 2 (by "Nanosizer" apparatus). GPC studies showed that 32% of the polyoxyalkylene chains were bonded to the surface.
Example 5
Preparation of particles of about 57 nm diameter, having a formulated core:sheath mass ratio of 92:8, the polyoxyalkylene chains having on average about 10 ethylene oxide units. This example uses a Type A seed-feed process (see Example 2).
The following materials and quantities were used
The method used was that of Example 2.
The result was a translucent dispersion of polymer particles. The weight solids of the dispersion was 51% and particle diameter was 57 nm (as measured by electron microscopy) 70 nm (polydispersity 3) (by "Nanosizer" apparatus) NMR studies showed that 45% of the polyoxyalkylene chains were covalently bonded to the particles.
Example 6
Preparation of particles of polymer of about 68 nm diameter, having a formulated core:sheath mass ratio of 90:10, the polyoxyalkylene chains having on average about 10 ethylene oxide units. In this example, there is used a seed-feed process wherein the seed stage is polymerised prior to the addition of the feed stage. This is hereinafter referred to as a "Type B" process.
The materials and total quantities of Example 2 were used, but with some differences as to the quantities used at particular stages in the process, as shall be apparent from the following description of the method.
The seed stage of Example 2, from which the t-butyl perbenzoate had been omitted, was cooled to 7.degree. C. and its pH adjusted to 3.0. To this cooled seed stage, 0.155 parts t-butyl perbenzoate 1.555 parts of Solution A and 0.155 parts of Solution B were added. Polymerisation commenced with this addition and the mixture was allowed to exotherm and then allowed to cool to room temperature. The remaining solution and t-butyl perbenzoate were added to the seed stage and the remaining Solution A was added to the feed stage and the feed stage was added over a period of 1 hour.
The resulting translucent dispersion of polymer particles had a weight solids content of 51% and the particle diameter, as measured by "Nanosizer" apparatus, was 68 nm (polydispersity 3).
Example 7
Preparation of particles of polymer of about 62 nm diameter having a formulated core:sheath mass ratio of 87:13, the polyoxyalkylene chains having on average about 15 ethylene oxide units. This example was a Type A seed-feed process (see Example 2) and sheath material is provided by ethoxylated undecylenic acid and ethoxylated methacrylic acid.
This example was identical to Example 3 except for the following alterations:
(a) the ethoxylated "Ocenol" 110-130 was replaced by the same quantity of an ethoxylated undecylenic acid, this having on average 17.5 ethylene oxide units per undecylenic acid molecule;
(b) the quantities of methyl methacrylate and butyl acrylate used were as follows:
The preparation was carried out as described in Example 2 and the product was a translucent dispersion of weight solids content 51%. The particle size, as measured by "Nanosizer" apparatus was 62 nm (polydispersity 5).
Example 8
Preparation of particles of polymer of 65 nm diameter, having a formulated core:sheath mass ratio of 87.5:12.5, the polyoxyalkylene chains having on average about 10 ethylene oxide units. In this example, there is used a seed-feed process of Type A (see Example 2) and there is used a single monomer (styrene).
The materials and quantities used were as follows:
The preparation was carried out as described in Example 3 and the product was a translucent dispersion of polymer particles of weight solids content 51%. The particle size, as determined by "Nanosizer" apparatus was 65 nm (polydispersity 3).
Example 9
Preparation of particles of polymer of 47 nm diameter having a formulated core:sheath mass ratio of 84:16, the polyoxyalkylene chains having on average about 10 ethylene oxide units. In this example, there is used as seed-feed process of Type A (see Example 2) and there is used a single monomer (butyl acrylate).
The materials and quantities used were as follows:
The preparation was carried out as described in Example 3 and the product was a translucent dispersion of polymer particles of weight solids content 45%. The particle size, as determined by "Nanosizer" apparatus was 47 nm (polydispersity 4).
Example 10
Preparation of particles of polymer of about 82 nm diameter having a formulated core:sheath mass ratio of 90:10, the polyoxyalkylene chains having on average about 10 ethylene oxide units. This example was a Type A seed-feed process and utilises an adhesion-promoting monomer.
The materials and quantities used were as follows:
Preparation of polyvinyl acetate particles of about 72 nm diameter, having a formulated core:sheath mass ratio of 87:13, the polyoxyalkylene chains having on average about 22 ethylene oxide units. In this example, a Type A seed-feed process (see Example 2) is used.
The materials and quantities used were as follows:
The preparation was carried out as described in Example 3 except that the feed stage was added over 2 hours, with half being added in the first 30 minutes.
The product was a translucent dispersion of polymer particles of weight solids content 52%. The particle diameter, as measured by "Nanosizer"apparatus, was 72 nm (polydispersity 3).
Example 12
Preparation of polymer particles of about 47 nm diameter, having a formulated core:sheath mass ratio of 75:25, the polyoxyalkylene chains having on average about 10.3 ethylene oxide units. In this example, a single stage process is used.
The materials and quantities used were as follows:
The method used for this preparation was identical to that of Example 1. The result was a translucent dispersion of polymer particles with weight solids content 50%. The particle diameter, as measured by "Nanosizer" apparatus, was 47 nm (polydispersity 3).
Example 13
Preparation of polymer particles of about 59 nm diameter, having a formulated core:sheath mass ratio of 90:10, the polyoxyalkylene chains having on average about 10 ethylene oxide units. In this example, an ionic initiation system was used.
Example 2 was repeated but with the t-butyl perbenzoate and solution A of that example replaced respectively by identical quantities of ammonium persulphate and a solution of 1 part sodium metabisulphite to 5 parts deionised water.
The product was a translucent dispersion of polymer. The weight solids of the dispersion was 51% and the particle diameter was 59 nm, polydispersity 4 as measured by "Nanosizer" apparatus.
Example 14
Preparation of a semi-gloss coating composition using an aqueous dispersion of polymer particles according to the invention.
The following materials and quantities were used:
The A stage materials were mixed and the B stage materials added thereto. The mixture was stirred for 15 minutes at high speed and the C stage materials were then added with moderate stirring.
The paint when applied exhibits good early water resistance, fast dry, excellent washability with conventional household cleaner, improved opacity over that exhibited by conventional systems, good adhesion to aged alkyl enamel and low odour.
The coating when applied exhibited a richer fuller finish compared to conventional waterborne systems, as a result of its higher volume solids. The coating had good brush, roller and spray application with good flowout of imperfections such as brush marks.
Claims
We claim:
1. Polymer particles of 100 nm maximum average diameter and having core-sheath structure, the core comprising addition polymer and being water insoluble and the sheath comprising polyoxyalkylene chains of average length of from 6 to 25 oxyalkylene units per chain, at least 20 percent of these chains being covalently bonded to the core and there being present on each core sufficient chains such that the mass ratio of core to sheath if from 98:2 to 60:40, said particles being obtained by initiating polymerisation at below 40.degree. C.
2. Polymer particles according to claim 1, wherein the average length of the polyoxylkylene chains is from 8 to 25 alkylene oxide units.
3. Polymer particles according to claim 1, wherein the average length of the polyoxyalkylene chains is from 10 to 25 alkylene oxide units.
4. Polymer particles according to any one of claim 1-3, wherein the mass ratio of core to sheath is from 95:5 to 85:15.
5. Polymer particles according to claim 1, wherein the average particle diameter is from 20-80 nm.
6. Polymer particles according to claim 1, wherein the average particle diameter is from 30-65 nm.
7. Polymer particles according to claim 1, wherein the polyoxyalkylene chains consist mainly of oxyethylene units with a minor proportion of oxyalkylene units selected from oxypropylene and oxybutylene units.
8. Polymer particles according to claim 1, wherein the polyoxyalkylene chains consist entirely of oxyethylene units.
9. Polymer particles according to claim 1, wherein at least 50% of the polyoxyalkylene chains are bonded to the core.
10. Polymer particles according to claim 1, wherein a maximum of polyoxyalkylene chains is bonded to the core.
11. Polymer particles according to claim 1, wherein polyoxyalkylene chains are provided by at least one alkoxylated diethylenically unsaturated fatty alcohol.
12. Polymer particles according to claim 1, wherein polyoxyalkylene chains are provided by alkoxylated monomer.
13. Polymer particles according to claim 12, wherein the alkoxylated monomer is ethoxylated methacrylic acid.
14. A stable aqueous dispersion of polymer particles according to claim 1.
15. A process for the preparation of core-sheath addition polymer particles of 100 nm maximum average diameter wherein the core is water insoluble comprising the polymerization of ethylenically unsaturated monomer in aqueous medium in the presence of solvated polyoxyalkylene chains which comprise hydrophobic moieties ("amphiphile"), at least some of which moieties comprise at least one ethylenic double bond such that the ethylenic double bond of those moieties comprising one such bond be in a pendant or terminal position, the polyoxyalkylene chains having a chain length of from 6-25 oxyalkylene units at least 20 percent of these chains being covalently bonded to the core and the mass ratio of monomer to polyoxyalkylene chains being from 98:2 to 60:40, and polymerisation being initiated at under 40.degree. C.
16. A process according to claim 15, wherein the polymerisation is initiated at a temperature below 20.degree. C.
17. A process according to claim 15, wherein the polymerisation is initiated at a temperature in the range of from 0.degree.-10.degree. C.
18. A process according to claim 15, wherein the mass ratio of monomer to amphiphile is from 50:50 to 92:8 and the mass ratio of monomer+amphiphile to water is from 20:80 to 60:40.
19. A process according to any one of claim 5-18, wherein the particles are formed in two stages, a seed stage and a feed stage, characterised in that (i) in the seed stage, the mass of monomer to amphiphile is from 80:20 to 20:80 and the monomer+amphiphile to water mass ratio is from 20:80 to 40:60 (ii) in the feed stage, the feed has a monomer to amphiphile mass ratio of from 75:25 to 99:1 and a monomer+amphiphile to water mass ratio of from 40:60 to 90:10; and (iii) the mass ratio of seed stage monomer to feed stage monomer is 1.20 maximum.
20. A process according to claim 19, wherein polymerisation is initiated at the seed stage to form a dispersion of seed polymer particles prior to addition of the feed stage.
21. A process according to claim 19, wherein polymerisation is initiated when addition of the feed stage commences.
22. A process according to any one of claim 19-21, wherein the monomer includes a proportion of alkoxylated addition monomer.
23. A process according to claim 22, wherein the alkoxylated addition monomer is ethoxylated methacrylic acid.
24. A process according to claim 22 wherein the alkoxylated addition monomer is used only in the feed stage.
25. A coating composition whose film-former is an aqueous dispersion of particles according to of claim 1.
Patent Citations (7)
Non-Patent Literature (2)
- Akashi et al, Journal of Polymer Science: Part A: Polymer Chemistry, "Graft Copolymers Having Hydrophobic Backbone and Hydrophilic Branches. IV. A Copolymerization Study of Water-Soluble Oligovinylpyrrolidone Macromonomers", vol. 27, 3521-3530, Sep. 1989.
- Miyauchi et al, Journal of Polymer Science: Part A: Polymer Chemistry, "Graft Copolymers Having Hydrophobic Backbone and Hydrophilic Branches. III. Synthesis of Graft Copolymers Having Oligovinylpyrrolidone as Hydrophilic Branch", vol. 26, 1561-1571, Jun. 1988.