Background of the Invention
The present invention relates to a material of joining ceramics and metal, and method of joining the same.
An active metal method has been used as one of methods for joining metals and shaped powder material, such as ceramics.
In this method, materials liable to react with ceramics, that is titanium (Ti) or zirconium (Zr) liable to react with oxygen and the like, are employed as a braze. The braze used in the active metal method is formed of an alloy based on titanium or zirconium. Especially, a Ti-Cu-Ag type alloy has been employed.
In the active metal method, the braze is placed between a metal and a ceramic material, to which high temperature and high pressure are applied. Thereafter, the material is cooled, so that a metal and ceramic material are joined together.
According to Japanese Laid-open Patent Application No. Sho 59-232693, a clad type i.e. Ti-Cu-Ag alloy, was proposed for joining ceramics with metals. In case metal and ceramics are joined by active metal method using Ti-Cu-Ag alloy, it shows excellent in adherence or joining ability. However, the strength at a joint reduces rapidly above 300.degree. C. because the braze contains silver having low melting point. Consequently, in case a ceramic product as stated above is used in a condition of high temperature, the above causes problems. Further, in the active metal method, high pressure must be applied in joining metal and ceramic.
An object of the invention is to provide a material of joining ceramics and metals, and a method thereof, which can solve the problems mentioned above and can join ceramics and metals without high pressure and can improve the thermal resistance at a joint.
Summary of the Invention
In accordance with the invention, a material for joining ceramics and metals comprises a nickel plate and a titanium copper type braze. The titanium-copper braze is placed adjacent to the ceramics, and the nickel plate is located outside the titanium-copper braze. Preferably, the thickness the nickel plate is about 1.5 mm.
After the titanium-copper braze and the nickel plate is placed between the ceramics and metal as stated above, these materials are heated for a desired period of time under vacuum condition.
By heating them under vacuum condition, titanium-copper-nickel acts as a braze, copper being diffused into the braze to reduce its concentration, so that the thermal resistance at a joint can be improved. The nickel plate operates as a braze as well as a stress cushioning or buffer material.
Experimental results show that the strength at the joint can be improved and it can be kept stable up to 600.degree. C. by selecting the thickness of the nickel plate, which is about 1.5 mm.
Brief Description of the Drawings
FIG. 1 is an explanatory side view of the invention for showing materials disposed between ceramics and a stainless steel plate;
FIG. 2 is a time table for showing a relation between temperature and time when joining the ceramics and the metal plate;
FIG. 3 is a table for showing a relation between flexural strength and thickness of a metal plate; and
FIG. 4 is a table for showing a relation between flexural strength and temperature.
Detailed Description of Preferred Embodiment
In FIG. 1, one example of the present invention is shown, wherein silicon nitride ceramics 1 and a stainless steel plate 2 (SUS 304) as metal are utilized. Joining materials are interposed between the ceramics 1 and the plate 2.
The joining materials comprise nickel (Ni) plates 4, 5, a tungsten (W) plate 3, a copper (Cu) foil 6, and a titanium (Ti) film 7. In particular, the tungsten plate 3 with a thickness of 1.0 mm, is interposed between the nickel plate 4 with a thickness of 1.0 mm and the nickel plate 5 with a thickness of 1.5 mm. The copper foil 6 with a thickness of 20 microns and the titanium film 7 with a thickness of 1.5 micron are situated between the ceramics 1 and the nickel plate 5 so that the titanium film 7 contacts the ceramics 1.
The joining materials are piled up and heated under a vacuum of 5.times.10.sup.-5 Torr. In FIG. 2, the heating condition is shown, wherein the abscissa is time T(second), and the ordinate is temperature (0.degree. C.). These materials are heated to 1,200.degree. C. (t.sub.1) at a temperature increase rate of 0.34 .degree. C./sec (t), which is kept for 0.06 Ks (kilo second) (T1), and cooled to 1,150.degree. C. (t.sub.2), which is kept for 0.6 Ks (T.sub.2), and again cooled to 1,100.degree. C. (t.sub.3), which is kept for 3.6 Ks (T.sub.3).
The ceramics 1 and the stainless steel plate 2 under this heating condition show four-point flexural strength of 200 MPa (Mega Pascal) and thermal resistance of 600 .degree. C.
In the present invention, a Ni-W-Ni layer, i.e. the tungsten plate 3 interposed between the nickel plates 4 and 5, absorbs or relaxes thermal stress to operate as a stress relaxing layer, and the nickel plate 5, the copper foil 6 and the titanium film 7 act as a Ni-Cu-Ti type braze.
In the joining method above, the temperature t.sub.3 (1,100.degree. C.) for time T.sub.3 (3.6 Ks) was maintained in order to improve, thermal resistance by accelerating diffusion of copper in the and reducing copper concentration.
In the present invention, the thickness of the nickel plate 5 between the copper foil 6 and the tungsten plate 3 is important, because the joining strength changes to a great extent by changing the thickness of the nickel plate 5. The relationship between the thickness of the nickel plate 5 and the joining strength is shown in FIG. 3, wherein the abscissa is the thickness of the nickel plate (mm), and the ordinate is the point flexural strength.
As shown in FIG. 3, in case the thickness of the nickel plate is in the range of 1.0 mm to 1.7 mm, four-point flexural strength is above 200 MPa. Preferably, the thickness of the nickel plate 5 is 1.5 mm.
According to the present invention, the thermal, resistance at a joint can be improved by using the Ni-Cu-Ti braze, which uses nickel and does not use silver. FIG. 4 shows the relationship between the joining strength and temperature in case of using a usual Ag-Cu-Ti braze and the Ni-Cu-Ti type braze according to the invention.
The braze according to the invention, as shown by a solid line A in FIG. 4, can maintain the four-point flexural strength of 200 MPa from room temperature to 600.degree. C., but in case of using the conventional braze, i.e. Ag-Cu-Ti braze, as shown by a broken dashed line B in FIG. 4, the four-point flexural strength reduces to below 200 MPa at 400 .degree. C., and reduces rapidly along increasing temperature.
The invention can improve operation efficiency and is applicable to ceramic products having complicated shape because high pressure is unnecessary when joining.
In the example as stated above, a stainless steel plate was used as metal, but the invention can naturally be applied to joining between ceramics and metals other than the stainless steel plate.
While the invention has been explained with reference to the specific embodiment of the invention, explanation is illustrative and the invention is limited only by the appended claims.