Background of the Invention
1. Field of the Invention
The present invention relates to a process for producing a platinum tunneling probe tip having a sharp point for use in FE-SEM, STM, and an ion beam electrode.
2. Description of the Related Art
The production of a tunneling probe tip having a sharp point by electropolishing has heretofore been conducted on tungsten, TiC, tantalum, etc. With respect to platinum, it is known that the polishing can be conducted by electrolysis with some cyanide solution (see FIG. 1).
However, with respect to the electropolishing of platinum, since the crystal grain of a platinum tunneling probe tip material is large as opposed to tungsten, TiC, tantalum, etc., the grain boundary is selectively polished, which raises problems with poor reproducibility, such as occurrence of scattering, in the shape due to the anisotropy of the crystal face with respect to the rate of polishing and difficulty in sharpening the point.
Summary of the Invention
It is the primary object of the present invention to provide a method of manufacturing a platinum tunneling probe tip having a sharp point always produceable in an identical form through elimination of the above-mentioned drawback.
In accordance with the present invention, there is provided a method of manufacturing a platinum tunneling probe tip comprising subjecting platinum material to a mechanical polishing, or to primary electropolishing with a sodium cyanide or potassium cyanide solution and subjecting the treated platinum material to secondary electropolishing milling with a mixed acid comprising sulfuric acid, nitric acid, and phosphoric acid.
In the above-described electropolishing, the point of a platinum tunneling probe tip material is sharpened to a certain extent by the first stage electrolysis with a sodium cyanide or potassium cyanide solution to be formed into a sharp point, and the point is further sharpened by the second stage electrolysis with a mixed acid, which makes it possible to produce a platinum tunneling probe tip with high reproducibility.
Brief Description of the Drawings
FIG. 1 is an exterior view of a platinum tunneling probe tip after electropolishing with a cyanide solution according to the prior art, and FIG. 2 an exterior view of a platinum tunneling probe tip after electropolishing with a mixed acid according to an example of the present invention.
Description of the Preferred Embodiments
The present inventors have made various studies on electropolishing of a platinum tunneling probe tip material and, as a result, have found that electrolysis with a mixed acid comprising sulfuric acid, nitric acid, and phosphoric acid can provide excellent polishing finish with less influence of crystal grin of the platinum tunneling probe tip material. In view of the fact that the platinum tunneling probe tip cannot be sharpened by the above electropolishing unless the tip has a point sharpened to a certain extent, the present invention adopted a two-stage electropolishing process in the electrolysis wherein the electropolishing with the above-described mixed acid is conducted after a primary electropolishing with a sodium cyanide or potassium cyanide solution.
The present invention will now be described in more detail with reference to the following examples.
Example 1
A 0.3 mm .phi.-pure platinum wire as a tunneling probe tip material was degreased and washed with water. Then, the point portion of the tunneling probe tip material was immersed in a KCN solution to conduct first-stage electropolishing.
(First-stage electrolysis conditions)
electrolyte: 1M KCN
electrolyzing voltage: 2-20 V AC
plate: platinum
electrolyzing time: 3-20 min
After washing with water, a second-stage electropolishing was conducted with the following mixed acid to produce a platinum tunneling probe tip having a sharp point.
(Second-stage electrolysis conditions)
Composition of electrolyte:
sulfuric acid: 1 volume
nitric acid: 1 volume
phosphoric acid: 1 volume
electrolyzing voltage: 2-20 V AC
plate: platinum
electrolyzing time: 1-60 min
In the electropolishing, it is possible to arbitrarily regulate the sharpness of the point of the tunneling probe tip by varying the electrolyzing voltage and time.
The platinum tunneling probe tip thus formed had a high point-reproducibility and exhibited a stable tunneling probe tip performance (see FIG. 2).
Example 2
A 0.3 mm .phi.-pure platinum wire as a tunneling probe tip material was degreased and washed with water. Then, the point portion of the tunneling probe tip material was immersed in a NaCN solution to conduct first-stage electropolishing.
(First-stage electrolysis conditions)
electrolyte: 1M NaCN
electrolyzing voltage: 2-20 V AC
plate: platinum
electrolyzing time: 3-20 min
After washing with water, second-stage electropolishing was conducted with the following mixed acid to produce a platinum tunneling probe tip having a sharp point.
(Second-stage electrolysis conditions)
Composition of electrolyte:
sulfuric acid: 1 volume
nitric acid: 1 volume
phosphoric acid: 2 volumes
electrolyzing voltage: 2-20 V AC
plate: platinum
electrolyzing time: 1-60 min
In the electropolishing, it is possible to arbitrarily regulate the sharpness of the point of the tunneling probe tip by varying the electrolyzing voltage and time.
As with the platinum tunneling probe tips formed in Example 1, the platinum tunneling probe tips thus formed had a high point reproducibility and exhibited a stable tunneling probe tip performance.
Example 3
A 0.3 mm .phi.-platinum tunneling probe tip material was subjected to a first-stage electropolishing with a KCN solution in the same procedure as that of Example 1, and then subjected to a second-stage electropolishing with the following mixed acid.
(Second-stage electrolysis conditions)
Composition of electrolyte:
sulfuric acid: 10%
nitric acid: 5%
phosphoric acid: 10%
electrolyzing voltage: 2-20 V AC
plate: platinum
electrolyzing time: 1-60 min
In the electropolishing, it is possible to arbitrarily regulate the sharpness of the point of the tunneling probe tip by varying the electrolyzing voltage and time.
As with the platinum tunneling probe tips formed in Example 1, the platinum tunneling probe tips thus formed had a high point reproducibility and exhibited a stable tunneling probe tip performance.
With respect to the electrolysis conditions according to the present invention, the concentration of the electrolyte for the first-stage electrolysis (sodium cyanide or potassium cyanide) may be in any range besides the concentration used in the above-described Examples so long as the other conditions are properly selected. However, the concentration of the electrolyte is preferably 0.3 to 5M from the viewpoint of the rate of polishing. Although it is preferred that the mixed acid be free from water and comprise sulfuric acid, nitric acid, and phosphoric acid, an excellent polishing effect can be attained as far as the mixed acid comprises at least 10% of sulfuric acid, at least 5% of nitric acid, and at least 10% of phosphoric acid. Further, it is also possible to conduct surface regulation through cathode electrolysis with an acid solution after the second-stage electropolishing according to the present invention.
In a preferred embodiment, the platinum base material comprises at least 99.9% of Pt and 0.005% or less of copper with the balance being unavoidable ingredients and has a crystal grain diameter regulated to 10 to 200 .mu.m from the viewpoint of removing the factors inhibiting the polishing to form the point of a tunneling probe tip with a crystal grain having a suitable size.
With respect to the method of producing a tunneling probe tip having a sharp point after a mechanical polishing or primary electropolishing for shaping a tunneling probe tip material into a macroscopic tunneling probe tip, a secondary electropolishing milling with a polishing solution composed of sulfuric acid nitric acid, and phosphoric acid is conducted.
Various elements besides Pt are present as unavoidable ingredients in the platinum material and they remarkably spoil the electropolishing performance through selective dissolution thereof during electropolishing, although this tendency depends upon the content and kind of the element. In particular, Cu has a large influence of this type, and it is therefore preferred that the Cu content be 0.005% or less.
The polishing solution comprising sulfuric acid, nitric acid, and phosphoric acid is suited for fine polishing, and it is difficult to directly shape a tunneling probe tip material into a tunneling probe tip form by making use of this polishing solution. Therefore, it is necessary to previously shape the tunneling probe tip material into a macroscopic tunneling probe tip form through mechanical polishing or electropolishing in a cyanide bath or the like.
Example 4
A 0.3 mm .phi.-platinum wire was prepared from a platinum material comprising at least 99.9% of Pt and 0.005% of Cu with the balance being unavoidable ingredients such as Mn, Mg, Fe, Zn, Pd, Au, Ag and Rh through a step of wire drawing. The platinum wire was heat treated in vacuo at 700.degree. C. for 30 min, and then gradually cooled to prepare a platinum tunneling probe tip material having a crystal grain diameter of 10 to 100 .mu.m. The platinum tunneling probe tip material was shaped by mechanical polishing into a macroscopic tunneling probe tip form having a polishing angle of 30.degree.. Thereafter, the shaped tunneling probe tip material was degreased and washed with water and then subjected to electropolishing with the following polishing solution.
Polishing solution:
sulfuric acid-nitric acid-phosphoric acid
(1:1:1)
Electrolysis conditions:
voltage: 2-20 V AC
time: 1-60 min
plate: platinum
The tunneling probe tip thus formed had a sharp point and exhibited excellent performance when used as a platinum tunneling probe tip for STM.
Example 5
A 0.3 mm .phi.-platinum wire was prepared from a platinum material comprising at least 99.9% of Pt and 0.0025% or less of Cu with the balance being unavoidable ingredients such as Mg, Mn, Fe, Zn, Pd, Au, Ag and Rh through a step of wire drawing. The platinum wire was heat treated in vacuo at 800.degree. C. for 30 min and then gradually cooled to prepare a platinum material having a crystal grain diameter of 10 to 150 .mu.m. The point portion of the platinum tunneling probe tip material thus prepared was immersed in the following polishing solution and subjected to electropolishing to shape the material into a macroscopic tunneling probe tip form.
Polishing solution:
1M KCN solution
Electrolysis conditions:
voltage: 2-20 V AC
plate: platinum
time: 3-20 min
Thereafter, the shaped tunneling probe tip material was washed with water, and subjected to electropolishing with a polishing solution comprising sulfuric acid, nitric acid and phosphoric acid in the same manner as that of Example 1.
The tunneling probe tip thus formed had a sharp point and exhibited excellent performance when used as a platinum tunneling probe tip for STM.
Example 6
Three kinds of 0.3 mm .phi.-platinum wires were prepared from platinum materials each having a Pt content of 99.9% and different in the contents of the remaining Cu and unavoidable ingredients (see Table 1) through a step of wire drawing.
The heat treatment, electropolishing with a potassium cyanide solution, and further electropolishing with a sulfuric acid-nitric acid-phosphoric acid solution were conducted by making use of the above-prepared platinum wires as the tunneling probe tip material in the same manner as that of Example 2. The shape of the point of each platinum tunneling probe tip thus formed was observed. As a result, it has been found that the tunneling probe tips prepared by using platinum materials each having a Pt content of 99.9% or more and a Cu content of 0.005% or less (materials A and B) according to the present invention had a very sharp point and exhibited excellent performance when used as a tunneling probe tip for STM. By contrast, the tunneling probe tip prepared by using a material having a Cu content exceeding 0.005% (material C) had no sharp point because of high rate of polishing.
Although the present embodiments were described with reference to the Examples wherein a polishing solution comprising sulfuric acid, nitric acid and phosphoric acid in a ratio of 1:1:1 was used, the same polishing performance can be attained when the polishing solution comprises at least 10% of sulfuric acid, at least 5% of nitric acid and at least 10% of phosphoric acid.
As described above, the present invention enables production of a platinum tunneling probe tip with a high reproducibility and a high point sharpness which has not been attained in the prior art.
The present invention exhibits a particularly excellent effect when used for the fabrication of a platinum tunneling probe tip for STM.