EXAMPLE 1
Into a 200-c.c. glass ampule were placed 50 g of a monomer represented by the formula: CH.sub.2 .dbd.CF--COOCH.sub.2 CF(CF.sub.3)OC.sub.3 F.sub.7 (hereinafter referred to as ".alpha.f6OF"), 4 g of glycidyl methacrylate (hereinafter referred to as "GMA"), 80 g of m-xylene hexafluoride (hereinafter referred to as "m-XHF") and 0.5 g of azobisisobutyronitrile, and the mixture was deaerated and purged with nitrogen repeatedly three times by the freeze-thaw method using methanol/dry ice. The ampule was then sealed off.
The ampule was immersed in a constant-temperature bath at 50.degree. C. for 30 hours.
The reaction mixture was thereafter placed into petroleum ether, and the resulting precipitate of fluorine-containing polymer was dried, giving 52 g of a fluorine-containing polymer.
The polymer had an intrinsic viscosity [.eta.] of 1.12 as measured at a temperature of 35.degree. C. using m-XHF as a solvent.
Elementary analysis of the polymer revealed 30.2% of carbon and 54.4% of fluorine, indicating that the monomers had been polymerized almost entirely.
The polymer was dissolved in m-XHF (dissolving solvent) to a concentration of 30 wt.%, and the solution was diluted with trichlorotrifluoroethane (diluting solvent) to a concentration of 0.5 wt.%.
The dilution was applied to a synthetic leather comprising a polyurethane-coated nonwoven fabric, 3 mm in thickness, with a brush and then heated at 80.degree. C. for 30 minutes to prepare a specimen for testing adhesion.
The contact angle of water, as well as n-hexadecane, with respect to the specimen was measured immediately after the preparation and after flexing the specimen through 120 degrees 10,000 times. Table 2 shows the results.
EXAMPLES 2-9 and COMPARATIVE EXAMPLES 1-3
Adhesion test specimens were prepared in the same manner as in Example 1 using the monomers, polymer dissolving solvent and diluting solvent listed in Table 1 for each polymer. Table 2 shows the results.
In Table 1 and in the following, the monomer representing symbols represent the following.
MA : CH.sub.2 .dbd.CHCOOCH.sub.3
.alpha.F17F : CH.sub.2 .dbd.CHCOOCH.sub.2 CH.sub.2 (CF.sub.2 CF.sub.2).sub.3 CF.sub.2 CF.sub.3
CMS : CH.sub.2 .dbd.CH--Ph--CH.sub.2 Cl (wherein Ph is phenylene)
SA : CH.sub.2 .dbd.CHCOOC.sub.18 H.sub.37
17FA : CH.sub.2 .dbd.CHCOOCH.sub.2 CH.sub.2 C.sub.8 F.sub.17
.alpha.Fi19F : CH.sub.2 .dbd.CFCOOCH.sub.2 CH.sub.2 (CF.sub.2 CF.sub.2).sub.3 CF(CF.sub.3).sub.2
EGMA : CH.sub.2 .dbd.C(CH.sub.3)COO(CH.sub.2 CH.sub.2 O).sub.3 COC(CH.sub.3).dbd.CH.sub.2
SMA : CH.sub.2 .dbd.C(CH.sub.3)COOC.sub.18 H.sub.37
17FMA : CH.sub.2 .dbd.C(CH.sub.3)COOCH.sub.2 CH.sub.2 C.sub.8 F.sub.17
19FA : CH.sub.2 .dbd.CHCOOCH.sub.2 CH.sub.2 C.sub.9 F.sub.19
EXAMPLE 10
Water (1.9 liters), 400 g of acetone, 300 g of .alpha. F6OF, 19 g of MA, 1 g of EGMA and 40 g of an emulsifier (K220, product of Nippon Oils & Fats Co., Ltd.) were placed into a 3-liter four-necked flask equipped with a stirrer, thermometer, reflux condenser and dropping funnel and oxygen was removed from the system by introducing nitrogen thereinto. The flask was placed into a constant-temperature bath at 65.degree. C. After the mixture was heated to a constant temperature, 0.1 liter of water having dissolved therein 1.6 g of azobisisobutyronitrile hydrochloride was added dropwise to the mixture to start polymerization.
Four hours later, a dispersion was obtained which contained 12 wt.% of solids. A portion of the dispersion was sampled and checked for monomer composition ratio and intrinsic viscosity [.eta.]. The .alpha.F6OF/MA/EGMA ratio was 97.3/6/0.3 by weight (elementary analysis: 39.6% carbon and 55.0% fluorine) and the viscosity [.eta.] was 0.68.
The dispersion was diluted with water to a concentration of 0.5 wt.% in a padding container. A polyester fabric was dipped in the padding bath, squeezed to remove the dilution, then dried at 80.degree. C. for 3 minutes and heat-treated at 150.degree. C. for 3 minutes to obtain a test specimen.
The specimen was tested for water repellency according to JIS L 1092 and for oil-repellency according to AATCC 118-1966T. The results were 100.sup.+ and No.6, respectively.
The same specimen as above was washed under the conditions of bath ratio of 1:50 and temperature of 40.degree. C. using a household electric washing machine and a detergent ("Super-Sabu", product of Kao Co., Ltd., Japan), then dried in air, lightly ironed at 140.degree. C. and subjected to the two tests againing, giving the results of 100.sup.+ and No.5, respectively.
COMPARATIVE EXAMPLE 4
Polymerization was conducted and a test specimen was prepared under the same conditions as in Example 10 with the exception of using 300 g of 17FA, 19 g of MMA and 1 g of EGMA as monomers. The polymer obtained was 0.38 in intrinsic viscosity [.eta.].
Under the same conditions as in Example 10, the specimen was tested for water repellency and for oil repellency before and after laundry. The water repellency reduced from 100+to 70, and the oil repellency from No.3 to No.0.
EXAMPLE 11
Into a 200-c.c. glass ampule were placed 30 g of a monomer represented by the formula: CH.sub.2 .dbd.CClCOOCH.sub.3, 20 g of a monomer of the formula: CH.sub.2 .dbd.C(CH.sub.3)COOCH.sub.2 CH.sub.2 C.sub.8 F.sub.17, 2 g of glycidyl methacrylate and 0.3 g of azobisisobutyronitrile, and the mixture was deaerated and purged with nitrogen repeatedly three times by the freeze-thaw method using methanol dry ice. The ampule was thereafter sealed off and immersed in a constant-temperature bath for 24 hours.
The reaction mixture was dissolved in 100 g of chloroform, and the mixture was placed into 2 liters of petroleum ether. The resulting precipitate was dried, giving 48 g of a fluorine-containing copolymer. The copolymer had an intrinsic viscosity [.eta.] of 1.06 as measured at a temperature of 35.degree. C. using chloroform as a solvent. Elementary analysis of the polymer revealed 37.4% of carbon, 17% of chlorine and 23.3% of fluorine, indicating that the monomers had been polymerized almost wholly.
The polymer was dissolved in chloroform (dissolving solvent) to a concentration of 5 wt.%, and the solution was diluted with 1,1,2-trichloro-1,2,2-trifluoroethane (diluting solvent) to a concentration of 0.5 wt.%.
Using the dilution, a specimen was prepared and tested for adhesion in the same manner as in Example 1. Table 4 shows the results.
EXAMPLES 12-15 and COMPARATIVE EXAMPLE 5
Adhesion test specimens were prepared in the same manner as in Example 11 using the monomers, dissolving solvent and diluting solvent listed in Table 3 for each polymer. The specimens were similarly tested with the results given in Table 4.
In Table 3, the monomer representing symbols mean the following monomers.
.alpha.ClS : CH.sub.2 .dbd.CClCOOC.sub.18 H.sub.37 ##STR14## .alpha.FS : CH.sub.2 .dbd.CFCOOC.sub.18 H.sub.37 17FMA : CH.sub.2 .dbd.C(CH.sub.3)COOCH.sub.2 CH.sub.2 C.sub.8 F.sub.17
19FA : CH.sub.2 .dbd.CHCOOCH.sub.2 CH.sub.2 (CF.sub.2 CF.sub.2).sub.3 CF(CF.sub.3).sub.2
17FA : CH.sub.2 .dbd.CHCOOCH.sub.2 CH.sub.2 C.sub.8 F.sub.17
19FMA : CH.sub.2 .dbd.C(CH.sub.3)COOCH.sub.2 CH.sub.2 (CF.sub.2 CF.sub.2).sub.3 CF(CF.sub.3).sub.2
.alpha.ClMe : CH.sub.2 .dbd.CClCOOCH.sub.3
EXAMPLE 16
Into a 3-liter four-necked flask equipped with a stirrer, thermometer, reflux condenser and dropping funnel were placed I.9 liters of water, 400 g of acetone, 150 g of butyl .alpha. -chloroacrylate, 150 g of 17FMA, 1 g of EGMA and g of an emulsifier (K220, product of Nippon Oils & Fats Co., Ltd.), and oxygen was removed from the system by introducing nitrogen thereinto. The flask was placed into a constant-temperature bath at 65.degree. C. After the mixture was heated to a constant temperature, 0.1 liter of water having dissolved therein 1.6 g of azobisisobutyronitrile hydrochloride was added dropwise to the mixture to start polymerization.
Four hours later, a dispersion was obtained which contained 12 2 wt.% of solids. A portion of the dispersion was sampled and checked for monomer composition ratio and intrinsic viscosity [.eta.]. The butyl .alpha.-chloroacrylate/17FMA/EGMA ratio was 49.9/49.8/0.3 by weight (elementary analysis: 41.7% carbon, 10.9% chlorine and 30.2% fluorine) and the viscosity [.eta.] was 0.50.
The dispersion was diluted with water to a concentration of 0.5 wt.% in a padding container. A polyester fabric was dipped in the padding bath, squeezed to remove the dilution, then dried at 80.degree. C. for 3 minutes and heat-treated at 150.degree. C. for 3 minutes to obtain a test specimen.
The specimen was tested for water repellency according to JIS L 1092 and for oil-repellency according to AATCC 118-1966T. The results were 100 and No.4, respectively.
The same specimen as above was washed under the conditions of bath ratio of 1:50 and temperature of 40.degree. C using a household electric washing machine and a detergent ("Super-Sabu", product of Kao Co., Ltd., Japan,)then dried in air, lightly ironed at 140.degree. C. and subjected to the above two tests with the results 90.sup.- and No.3, respectively.
COMPARATIVE EXAMPLE 6
Polymerization was conducted and a test specimen was prepared under the same conditions are in Example 16 with the exception of using 300 g of 17FA, 17 g of methyl methacrylate and 1 g of a monomer represented by the formula: CH.sub.2 .dbd.C(CH.sub.3)COO(CH.sub.2 CH.sub.20).sub.3 COC(CH.sub.3).dbd.CH.sub.2. The polymer obtained had an intrinsic viscosity [.eta.]of 0.38.
Under the same conditions as in Example 16, the specimen was tested for water repellency and for oil repellency before and after laundry. The water repellency reduced from 100.sup.+ to 70, and the oil repellency from No.3 to No.0.
EXAMPLE 17
One gram of the same fluorine-containing copolymer as used in Example 13 was dissolved in m XHF to a concentration 5 wt.%, and the solution was cast into a dish, 9 cm in diameter, and dried, giving a sheet, 100 .mu.m in thickness.
The rupture strength and elongation of the sheet were measured by an autograph (product of Shimadzu Seisakusho Ltd.), with the results of 0.7 kgf/mm.sup.2 and 320%, respectively.
COMPARATIVE EXAMPLE 7
A specimen was prepared and tested for rupture strength and elongation in the same manner as in Example 17 except that the fluorine-containing copolymer used in Example 11 was replaced by the polymer used in Comparative Example 5. The results were 0.26 kgf/mm.sup.2 and 450%, respectively.