COMPARATIVE EXAMPLE 1
In the same manner as of Example 1, pellets of polymer were produced under the conditions as shown in Table 3. Some fish eyes were seen on the surface of the pellets. Thus obtained pellets were injection molded and the resulting test pieces were subjected to the same tests as in Example 1 to obtain the results as shown in Table 3.
COMPARATIVE EXAMPLE 2
The latex of graft rubber polymer produced in Example 1 was coagulated with sulfuric acid by a conventional method and the obtained polymer wet powder was subjected to washing, dehydration and drying to obtain graft rubber polymer dry powder. This graft rubber polymer, the acrylonitrile-styrene copolymer produced in Example 1 and a slight amount of the additives used in Example 1 were mixed and formed into pellets by a screw extruder. The composition of these pellets was the same as that of the pellets obtained in Example 1, but there were many fish eyes on the surface. Thus, the pellets obtained in this Comparative Example had no value as commercial products. Furthermore, these pellets were injection molded and subjected to the same tests as in Example 1 to obtain the results as shown in Table 4.
EXAMPLES 5.8
A latex of graft rubber polymer was prepared using the same agents as in Example 1 in accordance with the formulation of Table 5.
60 parts of thus obtained latex of graft rubber polymer, the acrylonitrile-styrene copolymer used in Example 1 and in the amounts as shown in column 3 of Table 6, ethylbenzene in the amounts as shown in column 2 of Table 6 and 40 parts of a 1 wt% aqueous aluminum sulfate solution were mixed to obtain a mixture, which separated into two phases as in Example 1. After removal of the aqueous phase, using the acrylonitrile-styrene copolymer used in Example 1 in the amounts as shown in columns 4 and 5 of Table 6 was added to the organic phase and mixed, and pellets were produced in the same manner as in Example 1. The pellets had smooth surface and had no fish eyes. These pellets were injection molded to make various test pieces and properties thereof were measured in the same manner as in Example 1 to obtain the results as shown in Table 6. These results show that the rubber modified thermoplastic resins produced in these Examples were superior.
EXAMPLES 9-12
Methyl methacrylate and methyl acrylate were graft polymerized on SBR rubber latex of 0.14 .mu.m in average particle diameter in accordance with the formulation of Table 7 to obtain a latex of graft rubber polymer.
Polymethyl methacrylate as a thermoplastic resin (2) and a thermoplastic rein (3) was produced in accordance with the formulation of Table 8.
After completion of polymerization, the obtained suspension of polymethyl methacrylate was subjected to centrifugal dehydration and dried at 80.degree. C. to obtain a powder of the polymer.
Then, 90 parts of said latex of graft rubber polymer, chloroform in the amounts as indicated in column 2 of Table 9, said polymethyl methacrylate in the amounts as indicated in column 3 of Table 9 and 300 parts of a 0.1 wt% dilute aqueous magnesium sulfate solution were mixed. The mixture separated into an aqueous phase and a high viscous organic phase. Using the same device as in Example 1 and with addition of said polymethyl methacrylate powder in the amounts as shown in columns 4 and 5 of Table 9, the mixture was molded into pellets in the same manner as in Example 1. The surface of thus obtained pellets was smooth and there were no fish eyes. These pellets were injection molded to make various test pieces and properties thereof were measured to obtain the results as shown in Table 9. These results indicate that the rubber modified thermoplastic resins produced in these Examples were superior.
REFERENCE EXAMPLE
The pellets obtained in Example 2 were fed again through the first feed opening of the single-screw extruder of 30 mm.phi. and L/D=30 used in Example 2 and pellets were produced with drawing a vacuum of 160 Torr abs from the vent hole to try removal of toluen remaining in the pellets. (The second feed opening was closed.) Furthermore, thus obtained pellets were subjected to the said operation. This operation was repeated to examine the process of reduction of the amount of the remaining toluene. The results are shown in Table 10.
EXAMPLE 13
300 parts of the same latex of graft rubber polymer as used in Example 1, 50 parts of the same acrylonitrile-styrene copolymer powder as used in Example 1 [thermoplastic resin (2) at step (I)], 240 parts of toluene, 1000 parts of a 0.1 wt % dilute aqueous sulfuric acid solution, 0.25 part of Irganox 1076 and 1.25 parts of Armide HT were mixed. The resulting mixture separated into an aqueous phase and a high viscous organic phase. The organic phase was passed between two press rollers to remove the remaining aqueous phase, followed by adding said molding assistant in the same amount as above. This was fed from the first feed opening of a vented extruder having the first feed opening, vent hole and the second feed opening and toluene was devolatilized from the vent hole and then 100 parts of said copolymer powder [thermoplastic resin (3) at step (V)] was continuously fed from the second feed opening and melt mixed with the polymer fed from the first feed opening to mold the polymer into pellets. The resulting pellets contained 16.0% by weight of polybutadiene and had smooth surface with no fish eyes. These pellets were injection molded to make various test pieces and properties thereof were measured to obtain the results as shown in Table 11. These results show the superiority of the rubber modified thermoplastic resin produced in this Example.
EXAMPLE 14
60 parts of the latex of graft rubber polymer used in Example 5, 20 parts of acrylonitrile-styrene copolymer [thermoplastic resin (2) at step (I)] used in Example 1, 25 parts of ethylbenzene and 40 parts of 1 wt % aluminum sulfate were mixed to obtain a mixture, which separated into the two phases as in Example 13. This was subjected to dehydration and devolatilization in the same manner as in Example 13 and then was melt mixed with 60 parts of said acrylonitrile-styrene copolymer [thermoplastic resin (3) at step (V)] and the mixture was moled into pellets. Thus obtained pellets contained 16.0% by weight of polybutadiene and had smooth surface and had no fish eyes. These pellets were injection molded to make various test pieces. Properties of these test pieces were measured by the same procedures as in Example 1 to obtain the results as shown in Table 12. These results indicate the superiority of the rubber modified thermoplastic resin produced in this Example.
EXAMPLE 15
90 parts of the latex of graft rubber polymer used in Example 9, 20 parts of polymethyl methacrylate powder [thermoplastic resin (2) at step (I)] used in Example 9, 50 parts of chloroform and 300 parts of a 0.1 wt % dilute aqueous magnesium sulfate solution were mixed to obtain a mixture which separated into an aqueous phase and a high viscous organic phase. Removal of the aqueous phase and devolatilization of chloroform were carried out by the same device as used in Example 13 and in the same manner as in Example 13, followed by melt-mixing 50 parts of said polymethyl methacrylate powder [thermoplastic resin (3) at step (V)] and pelletization. Thus obtained pellets contained 14.9% by weight of a rubber polymer and had a smooth surface and had no fish eyes. Then, these pellets were injection molded to make various test pieces and properties of the test pieces were measured in the same manner as in Example 9 to obtain the results as shown in Table 13. These results show the superiority of the rubber modified thermoplastic resin obtained in this Example.
EXAMPLE 16
37.5 parts of the latex of graft rubber polymer obtained in Example 5 and 7 parts of a 1 wt % aqueous sulfuric acid solution were fed from a first feed opening to a twin-screw extruder having a first feed opening, a second feed opening, a dehydrating part, a devolatilizing part and a third feed opening. This mixture converted to creamy state before it reached to the second feed opening and separated into an aqueous phase and a high viscous organic phase when 25 parts of dichloromethane and 12.5 parts of the acrylonitrile-styrene copolymer [thermoplastic resin (2) at step (I)] used in Example 1 were added continuously from the second feed opening. Then, the aqueous phase was discharged from the dehydrating part and dichloromethane was devolatilized from the devolatilizing part and thereafter 75 parts of a polycarbonate resin (Novalex 7022 manufactured by Mitsubishi Chemical Industries Ltd.) [thermoplastic resin (3) at step (V)] was continuously added from the third feed opening to melt-mix with the graft rubber polymer and the acrylonitrile-styrene copolymer. The resulting mixture was molded into pellets by extruding from a nozzle. The pellets contained 10.0% by weight of polybutadiene and had no fish eyes. The pellets were injection molded to make standard test pieces and the test results on these test pieces are shown in Table 14 (Measurements were conducted in the same manner as in Example 1).
EXAMPLE 17
When 300 parts of the latex of graft rubber polymer used in Example 1, 40 parts of the acrylonitrile-styrene copolymer powder [thermoplastic resin (2) at step (I)] used in Example 1, 200 parts of toluene, 1000 parts of a 0.1 wt % dilute aqueous sulfuric acid solution, 0.25 part of Irganox 1076 and 1.25 parts of Armide HT were mixed, the resulting mixture separated into an aqueous phase and a high viscous organic phase. The organic phase was passed between two press rolls to remove remaining aqueous phase and fed from a first feed opening of an extruder having two feed openings for resin and two vent holes and having no special mixing mechanism. A part of toluene contained in the polymer was devolatilized from the first vent hole, 110 parts of said copolymer powder [thermoplastic resin (3) at step (V)] was fed from the second feed opening provided just behind the first vent hole, the remaining toluene was devolatilized from the second vent hole provided down the second feed opening and the polymer was molded into pellets. The proportion of the amounts of toluene devolatilized from the first vent and the second vent was about 3:2. The surface of thus obtained pellets was smooth and there were no fish eyes. These pellets were injection molded to make various test pieces and properties thereof were measured in the same manner as in Example 1 to obtain the results as shown in Table 15. These results show that the rubber modified thermoplastic resin produced in this Example was superior.
EXAMPLE 18
60 parts of latex of graft rubber polymer used in Example 5, 30 parts of the acrylonitrile-styrene copolymer [thermoplastic resin (2) at step (I)] used in Example 1, 40 parts of ethylbenzene and 40 parts of 1 wt % magnesium sulfate were mixed by a continuous kneader. The resulting mixture separated into two phases as in Example 17. This was continuously fed to an extruder having successively a first feed opening, a dehydration part, a first devolatilizing part, a second feed opening and a second devolatilizing part and was subjected to dehydration and first devolatilization, then 71 parts of the acrylonitrile-styrene copolymer [thermoplastic resin (3) at step (V)] used in Example 1 was fed from the second feed opening, second devolatilization was carried out and the polymer was molded into pellets. The proportion of amount of ethylbenzene devolatilized by the first devolatilization and the second devolatilization was about 1:1. The surface of the obtained pellets was smooth and no fish eyes were seen. These pellets were injection molded to make various test pieces and properties thereof were measured to obtain the results as shown in Table 16. These results indicate the superiority of the rubber modified thermoplastic resin produced in this Example.
EXAMPLE 19
When 90 parts of the latex of graft rubber polymer used in Example 9, 10 parts of the polymethyl methacrylate powder [thermoplastic resin (2) at step (I)] used in Example 9, 20 parts of chloroform and 300 parts of a 0.2 wt % dilute aqueous magnesium sulfate solution were continuously mixed, the resulting mixture separated into an aqueous phase and a high viscous organic phase. This mixture was subjected to removal of the aqueous phase and first devolatilization of chloroform by the same device as used in Example 18, successively 60 parts of said polymethyl methacrylate powder [thermoplastic resin (3) at step (V)] was continuously fed from a feed opening provided at the device to carry out melt kneading, then second devolatilization was further carried out and thereafter the polymer mixture was molded into pellets. Thus obtained pellets had smooth surface and had no fish eyes. These pellets were further injection molded to make various test pieces and properties thereof were measured in the same manner as in Example 9 to obtain the results as shown in Table 17. These results show the superiority of the rubber modified thermoplastic resin produced in this Example.
EXAMPLE 20
37.5 parts of the latex of graft rubber polymer obtained in Example 5 and 7 parts of 1 wt % aqueous sulfuric acid solution were continuously fed from a first feed opening of a twin-screw extruder having a first feed opening, a second feed opening, a dehydrating part, a first devolatilizing part, a third feed opening and a second devolatilizing part. This mixture converted to creamy state before reaching the second feed opening and when 10 parts of dichloromethane and 12.5 parts of the acrylonitrile-styrene copolymer [thermoplastic resin (2) at step (I)] used in Example 1 were continuously fed from the second feed opening, the resulting mixture separated into an aqueous phase and a high viscous organic phase. The aqueous phase was discharged from the dehydrating part and a part of dichloromethane was devolatilized from the first devolatilizing part, followed by continuously feeding 75 parts of a polycarbonate resin (Novalex 7022 manufactured by Mitsubishi Chemical Industries Ltd.) [thermoplastic resin (3) at step (V)] from the third feed opening to melt-mix with the mixture of the graft rubber copolymer and the acrylonitrile-styrene copolymer and then devolatilizing the remaining dichloromethane from the second devolatilizing part. The proportion of the amount of dichloromethane devolatilized from the first devolatilizing part and the second devolatilizing part was about 1:4. The mixture thus obtained was molded into pellets by extruding from a nozzle. These pellets contained 10.0% by weight of polybutadiene and had no fish eyes. These pellets were injection molded to make standard test pieces and the test results on these test pieces are shown in Table 18. (Test methods were the same as in Example 1.)
EXAMPLES 21-25
When 300 parts (100 parts in terms of solid matter) of the latex of graft rubber polymer used in Example 1, toluene in the amounts as indicated in column 2 of Table 19, 1000 parts of a 0.1 wt % dilute aqueous sulfuric acid solution and 0.1% by weight (based on the weight of all the polymers) of an aging resister (Irganox 1076) and 0.5% by weight (based on the weight of all the polymer) of a molding assistant (Armide HT) were mixed at 70.degree. C. for 5 minutes by a 10 l batch type kneader, the resulting mixture separated into an aqueous phase and a high viscous organic phase. When the aqueous phase was removed, followed by adding an acrylonitrile-styrene copolymer used in Example 1 in the amounts as shown in column 3 of Table 19 and mixing and kneading at 70.degree. C. for about 10 minutes, the organic phase became a soft particulate material of about 1 mm-5 mm in diameter and each particle was in such a state that said high viscous material and said copolymer powder were homogeneously mixed. To this particulate material was further added the acrylonitrile-styrene copolymer powder used in Example 1 in the amounts as shown in column 4 of Table 19 and these were mixed for about 2 minutes to obtain a particulate material comprising a dispersion of said copolymer powder in said particulate material. The resulting particulate material was molded into strands by a twin-screw granulating machine, which were cut by a pelletizer into pellets. To these pellets was added said molding assistant in the same amount as above and the mixture was fed from a first feed opening of a single-screw extruder of 30 mm.phi. and L/D=30 which had two feed openings and one vent and toluene and remaining water were removed from the vent, then the acrylonitrile-styrene copolymer powder used in Example 1 in the amounts as shown in column 5 of Table 19 was fed from the second feed opening to carry out melt-mixing and the mixture was discharged from the die at the tip of the extruder as strands. The resulting strands were cut by a pelletizer to obtain the objective pellets. Thus obtained pellets had a smooth surface and there were no fish eyes. They were injection molded to make various test pieces and properties thereof were measured in the same manner as in Example 1 to obtain the results as shown in Table 19. These results indicate that the rubber modified thermoplastic resin obtained in this Example was superior.
EXAMPLES 26-30
When 60 parts (20 parts in terms of solid matter) of the latex of graft rubber polymer used in Example 5, ethylbenzene in the amounts as shown in column 2 of Table 20 and 40 parts of 1% aqueous aluminum sulfate solution were mixed, the resulting mixture separated into two phases as in Example 21. The aqueous phase was removed and the remainder was treated in the same manner as in Example 21 using the acrylonitrile-styrene copolymer used in Example 1 in the amounts as shown in columns 3, 4 and 5 of Table 20 and molded into pellets. The surface of the pellets was smooth and they had no fish eyes. These pellets were injection molded to make various test pieces and properties thereof were measured in the same manner as in Example 1 to obtain the results as shown in Table 20. These results show the superiority of the rubber modified thermoplastic resin produced in these Examples.
EXAMPLES 31-35
90 parts (30 parts in terms of solid matter) of the latex of graft rubber polymer used in Example 9, chloroform in the amounts as shown in column 2 of Table 21 and 300 parts of 0.1 wt % aqueous magnesium sulfate solution were mixed to obtain a mixture which separated into an aqueous phase and a high viscous organic phase. The mixture was treated by the device used in Example 21 in the same manner as in Example 21 with addition of the polymethyl methacrylate powder used in Example 9 in the amounts as shown in columns 3, 4 and 5 of Table 21 and the mixture obtained was molded into pellets. These pellets had a smooth surface and no fish eyes were found. These pellets were injection molded to make test pieces and properties thereof were measured in the same manner as in Example 9 to obtain the results as shown in Table 21. These results means that the rubber modified thermoplastic resins were superior.
EXAMPLES 36 and 37
A latex of graft rubber polymer was prepared with the formulation of Table 22 using the same agents as in Example 1.
Grafting rate on the polybutadiene in thus obtained latex of graft rubber polymer was 40% and the graft rubber polymer contained 58 parts of single polymer.
When 160 parts (53 parts in terms of solid content) of this latex of graft rubber polymer, toluene in the amounts as shown in column 2 of Table 23, 1000 parts of 0.1 wt % dilute sulfuric acid and the same aging resister and the same molding assistant in the same amounts as those used in Example 21 were mixed, the resulting mixture separated into two phases as in Example 21 and was treated in the same manner as in Example 21 using the same acrylonitrile-styrene copolymer as in Example 1 in the amounts as shown in columns 3, 4 and 5 of Table 23 to obtain pellets.
Thus obtained pellets were smooth in surface and had no fish eyes. These pellets were injection molded to make test pieces and properties thereof were measured in the same manner as in Example 1 to obtain the results as shown in Table 23.
The advantage of the process of this invention in comparison with conventional processes is that the polymers need not be powdered. Further advantages are as follows:
(1) Dehydration and drying after production of wet powder by coagulation of latex and air transportation and storage of powder can be omitted. Thus, simplification of process is possible.
(2) Heat loss in dryer can be avoided. Cost can be reduced.
(3) Dust is not formed and working atmosphere is not polluted.
(4) According to this invention, a graft rubber polymer is dispersed in a thermoplastic resin in the presence of an organic agent and so the particles of graft rubber polymer do not coalesce with each other and homogeneous dispersion of the particles becomes possible. Thus, it is possible to produce rubber modified thermoplastic resin superior in quality to those produced by conventional processes.
(5) It is possible to produce rubber modified thermoplastic resin free from fish eyes, etc. which causes poor appearance of the products.
Furthermore, according to this invention, time of addition of the thermoplastic resin and effect of use of the thermoplastic resin are analyzed in detail to result in the following effects.
(6) Amount of the organic agent used can be reduced.
(7) Volumetric efficiency of the device can be improved.
That is, this invention provides the technique for producing rubber modified thermoplastic resins of high quality at low cost.