The explosion-welding of pipe joints in pipeline systems is of great interest, because welding operations can be carried out quickly and reliably, and without being dependent on external energy sources, such as electricity or gas.
Many different pipe joints have been developed and made the subject of patent applications over the passage of years.
Several of these known pipe joints, however, have been found to produce undesirable defects, such as non-bonded regions at the ends of the pipes, cold-work hardening or surface damage, all of which represent locations for potential attack by corrosion.
The pipe joint proposed in accordance with the present invention provides a complete bond and produces very little cold-working hardening and results in no surface damage.
Furthermore, as distinct from other known types of pipe joint which have two welds, the inventive pipe joint has only one weld, and no additional material need be added.
Description
The joint construction is illustrated in the accompanying drawing. The reference numeral 1 and 2 in the drawing identify the ends of two pipes to be welded together. The end 1 of one pipe has been chamfered internally, down to an angle of 12.degree. to 17.degree.preferably 15.degree., whereas the end 2 of the other pipe, e.g., the end of a pipeline, has been pressed out to a conical configuration, to form a cone angle of 5.degree. to 20.degree., preferably 10.degree., a cone angle of 5.degree. being shown in the drawing.
The explosive welding charge, 3, is a moulded charge which consists of an explosive, such as PETN, HMK or RDX, bound in a silicone rubber matrix. An addition of iron powder and glass spheres or beads is also included, additional to the explosive. The composition of the charge is adapted to obtain a detonation velocity of from 3700 m/s to 4300 m/s, preferably 3900 m/s.
The reference 4 identifies a plastic capsule which has the shape illustrated and which ensures that the explosive charge is positioned correctly in relation to the pipe ends and also that the charge has precise dimensions.
The charge is detonated by a charge detonating disc 5 which comprises an explosive substance of high brisance (a high crushing effect), e.g. PETN, RDX or HMX, bonded with silicone oil, plastic or latex, although such that the explosive substance equals at least 70% of the weight of the charge. This is necessary in order to produce detonation pressure which will suffice to fully detonate the explosive welding charge and to cause detonation in thin strata, or layers, so as to be able to minimize the total amount of charge.
The plastic capsule 4, and therewith the welding charge 3 has an axial extension, such as to enable detonation to reach a stable state before the detonation front reaches the point of the chamfered pipe end 1.
In this respect, the distance from the detonation disc to the chamfer point of the pipe end is at least 5 mm, preferably at least 6 mm. If one initiates firing of the detonating disc at its center, a full, axially directed detonation of the explosive welding charge can be realized.
This will result in the establishment of a complete bond at the point of said chamfered pipe end and therewith avoid the possibility of cavity corrosion.
The reference numeral 7 shown in the drawing identifies a fracture indication in the form of an annular external groove ground in the pipe material at least 10 mm from the extremity of pipe end 2. When the shock wave reflected from the pipe end 2 reaches the location of the groove, the pipe material will shear-off peripherally therearound. The sheared part of the pipe will therefore function as a wave trap and a complete bond will be obtained on the remaining part of the pipe. Those experiments carried out in order to establish suitable angles between the inner surface of the cone part of pipe end 2 and the rectilinear outer surface of pipe end 1, showed that an angle of 5.degree. will provide very good and reproduceable welds on ferritic stainless pipes of Duplex type.
In the case of more-readily welded materials, coned angles of pipe end 2 down to 3.degree. can be used without jeopardizing reproduceability of a satisfactory welded joint. A chamfer angle of 15.degree. has been found to produce good binding results at the pointed end of the pipe end 1. Although chamfer angles of pipe end 1 smaller than 15.degree. are fully acceptable, they require unnecessarily long charge lengths, without affording appreciable improvement of the result.
Angles larger than 15.degree. give inferior reproduceability of the bond at the point of the chamfered extremity of pipe end 1.