Abstract
A niobium-activated yttrium tantalate x-ray phosphor which incorporates small molar amounts of a rubidium or cesium halide, a strontium or barium halide, and, optionally, a gallium or aluminum oxide, to effect improved brightness.
Metadata
Assignee
- GTE Products Corporation
Inventor
- V. Butchi Reddy
Application Information
Application Number:US 4598911
Filing Date:1990-01-02
Priority Date:1990-01-02
Art Unit:113
Classifications
IPC:
C09K 1178
Field of Search:
252301.4 R;304.4 H
Patent Drawings
This patent does not have any drawings.
Description
TECHNICAL FIELD
This invention relates to the manufacture of niobium-activated yttrium tantalate x-ray phosphors.
BACKGROUND ART
Such phosphors are disclosed in U.S. Pat. Nos. 4,225,653 and 4,387,141. In both patents the phosphor composition has the formula YNb.sub.x Ta.sub.1-x O.sub.4, where x is 0 to about 0.15.
It has been discovered that phosphor brightness can be improved by the addition of small molar amounts of a halide of rubidium, cesium, strontium, or barium, and, optionally, an oxide of gallium or aluminum.
SUMMARY OF THE INVENTION
It is an object of the invention to provide a niobium-activated yttrium tantalate x-ray phosphor with improved brightness.
This object is accomplished, in one aspect of the invention, by a phosphor made by forming a uniform mixture of the following ingredients in the following proportions: one mole of yttrium oxide, 0.995 moles of tantalum oxide, 0.005 moles of niobium oxide, 0.001 moles of a halide of rubidium or cesium, 0.01 moles of a halide of strontium or barium, and, optionally, 0.01 moles of an oxide of gallium or aluminum, blending this mixture with a lithium chloride-lithium sulfate eutectic flux, and firing the mixture at about 1200.degree.-1300.degree. C. (2192.degree.-2372.degree. F.) for about 10-12 hours.
The following non-limiting examples are presented.
EXAMPLE 1 (Control)
One mole of yttrium oxide, Y.sub.2 O.sub.3, 0.995 moles of tantalum oxide, Ta.sub.2 O.sub.5, and 0.005 moles of niobium oxide, Nb.sub.2 O.sub.5, were weighed and blended together to form a phosphor composition of YTa.sub.0.995 Nb.sub.0.005 O.sub.4. The molar concentration of niobium activator was 0.005 moles. A flux of lithium chloride in an amount of 33 weight percent was added to the mixture and blended using standard blending procedures. The blend was loaded into an alumina crucible and fired in an electric furnace for about 10 to 12 hours at about 1200.degree.-1300.degree. C. (2192.degree.-2372.degree. F.). The fired material was cooled in the furnace and the flux material leached out with deionized water washings. The flux-free material was then filtered, dried and classified. The sample was then measured for luminescence efficiency under x-ray excitation. This sample was the control for the following examples and the brightness value was normalized at 100.
EXAMPLE 2
The procedure of Example 1 was followed using a eutectic flux mixture of lithium chloride and lithium sulfate, (LiCl).sub.2 -Li.sub.2 SO.sub.4 (46.5:53.5 mole percent, respectively), in an amount of 33 weight percent of the phosphor raw material. The eutectic temperature of this flux composition is about 478.degree. C. (892.degree. F.). This sample was 8% brighter than the control.
EXAMPLE 3
The procedure of Example 1 was followed, with the addition of 0.01 moles of strontium fluoride, 0.001 moles of rubidium chloride, and 0.01 moles of gallium oxide as dopants. A lithium chloride-lithium sulfate eutectic flux mixture, 33 weight percent, was used. This sample was 22% brighter than the control.
EXAMPLE 4
The procedure of Example 3 was repeated to determine reproducibility of the results. This sample was 20% brighter than the control.
EXAMPLE 5
The procedure of Example 3 was used, except that instead of 0.01 moles of gallium oxide, 0.01 moles of aluminum oxide was used. This sample was 16% brighter than the control.
EXAMPLE 6
The procedure of Example 5 was repeated to determine the reproducibility of the results. This sample was 18% brighter than the control.
EXAMPLE 7
The procedure of Example 3 was used, except that no gallium oxide was used. This sample was 12% brighter than the control.
X-ray optical fluorescence (XOF) brightness data for the examples are given in Table I.
While there has been shown and described what are at present considered the preferred embodiments of the invention, it will be obvious to those skilled in the art that various changes and modifications may be made therein without departing from the scope of the invention as defined by the appended claims.
Claims
What is claimed is:
1. A niobium-activated yttrium tantalate x-ray phosphor containing rubidium halide or cesium halide, strontium halide or barium halide and, optionally, gallium oxide or aluminum oxide incorporated therein, made by forming a uniform mixture of the following ingredients in the following proportions: one mole of yttrium oxide; 0.995 moles of tantalum oxide; 0.005 moles of niobium oxide; 0.001 moles of rubidium halide or cesium halide; 0.01 moles of strontium halide or barium halide; and, optionally, 0.01 moles of gallium oxide or aluminum oxide; blending said mixture with a lithium chloride-lithium sulfate eutectic flux composition; firing said mixture at about 1200.degree.-1300.degree. C. for about 10-12 hours to form said phosphor; washing said phosphor in deionized water to remove said flux; and filtering, drying and classifying said phosphor, said phosphor exhibiting a higher brightness than the phosphor prepared as above absent rubidium halide, cesium halide, strontium halide, barium halide, gallium oxide and aluminum oxide.
2. The phosphor of claim 1 wherein said halide is selected from the group consisting of chloride, fluoride, and bromide.
3. The phosphor of claim 1 wherein said eutectic flux composition comprises about 33 weight percent of said mixture.
4. The phosphor of claim 1 wherein said uniform mixture comprises one mole of yttrium oxide, 0.995 moles of tantalum oxide, 0.005 moles of niobium oxide, about 0.01 moles of strontium fluoride, about 0.001 moles of rubidium chloride, and about 0.01 moles of gallium oxide.
5. A method of making a niobium-activated yttrium-tantalate x-ray phosphor, comprising the steps of: forming a uniform mixture of the following ingredients in the following proportions: one mole of yttrium oxide, 0.995 moles of tantalum oxide, 0.005 moles of niobium oxide, 0.001 moles of cesium halide or rubidium halide, 0.01 moles of strontium halide or barium halide, and, optionally, 0.01 moles of gallium oxide or aluminum oxide; blending said mixture with a lithium chloride-lithium sulfate eutectic flux composition; and firing said mixture at about 1200.degree.-1300.degree. C. for about 10-12 hours to form said phosphor; washing said phosphor in deionized water to remove said flux; and filtering, drying and classifying said phosphor, said phosphor exhibiting a higher brightness than the phosphor prepared as above absent rubidium halide, cesium halide, strontium halide, barium halide, gallium oxide and aluminum oxide.
6. The method of claim 5 wherein said eutectic flux composition comprises about 33 weight percent of said mixture.