Example 1
A liquid reservoir composition was prepared by simply mixing together 30 parts of a diacrylate of a diglycidyl ether of bisphenol A having a number average molecular weight of 500, 30 parts of the diacrylate of neopentyl glycol propoxylated with 2 propylene oxide units per molecule, 20 parts of trimethylol propane trimethacrylate, 10 parts of N-vinyl pyrrolidone, and 10 parts of the diester adduct of acrylic acid with polymethylene glycol having a number average molecular weight of 1600. This liquid composition was rendered sensitive to ultraviolet light by mixing in 4% by weight of the composition being sensitized of a benzylketal photointiator (hydroxycyclohexyl phenyl ketone -- the Ciba-Geigy product Irgacure 184 may be used). The viscosity of this sample was 360 centipoises at room temperature (72.degree. F.).
The above liquid reservoir composition was exposed to the previously described helium-cadmium laser focused to 350 micron diameter at various velocities using one, two, or more passes to determine the effects. The results are presented in Table I below.
It can be seen from comparison of samples C and E that an equal total dose when applied in short repeated scans results in lower methyl ethyl ketone (MEK) extractables, improved physical strength, and a 50% reduction in the measured distortion of the previously described cantilevered rectangle. The same applies to samples D and G with respect to methyl ethyl ketone extractables and physical properties. Comparison of samples D, E and F show reduced methyl ethyl ketone extractables in multiscanned systems even though the total applied dosage is less than in the single scanned sample.
Of possible overriding importance is the distortion factor which was described previously and which is the ratio of the top of a thin cantilevered rectangle to the bottom of that same rectangle. Using the 0.315 sec/cm single exposure described previously, the distortion factor was 1.6 which indicates the top of the rectangle was 60% longer than its bottom. Using two 0.1575 sec/cm scans (for the same total of 0.315 sec/cm), the distortion factor was improved from the previous 1.6 to 1.3. More particularly, the top of the rectangle was now only 30% longer than its bottom, instead of being 60% longer. This provides a 50% reduction in the measured distortion using the same total exposure dosage.
Example 2
In a second example to show the effectiveness of short repeated scans in reducing the distortion factor, a liquid reservoir composition was prepared by simply mixing together 30 parts of a diacrylate ester of an ethoxylated bisphenol A having a number average molecular weight of 424, 20 parts of the diacrylate ester of a polymethylene glycol having a number average molecular weight of 1600, 25 parts of the diacrylate of neopentyl glycol propoxylated with two propylene oxide units per molecule, and 25 parts of N-vinyl pyrrolidone. This liquid composition was also rendered sensitive to ultraviolet light by mixing in 4% by weight of Irgacure 184 from Ciba-Geigy. The viscosity of this sample was 150centipoises at room temperature (72.degree. F.).
The above liquid reservoir composition was exposed to the previously described helium-cadmium laser focused to 350 micron diameter at various velocity using one, two, or more scans to produce the cantilevered rectangle as previously described for the measurement of distortion factors. The results are presented in Table II below.
After the photoformed object is removed from the liquid reservoir, the object is drained, sometimes rinsed, and then further cured, as desired, to increase its strength, but this is itself known.
To further illustrate the results obtainable in this invention, several different liquid reservoir compositions were formulated as follows:
As will be evident, composition B is more fluid and faster curing than composition A, and composition C is more fluid and faster curing than composition B. The viscosities are Brookfield Viscosities measured at 72.degree. F.
The distortion factor of each composition was measured using a single scan and the expected result was obtained, namely, the more fluid and faster curing the composition, the greater the distortion factor. More particularly, the distortion factor for the three compositions was determined using a single scan, all being scanned at the same rate to provide the same dosage. The distortion factor for composition A was 1.47, for composition B it was 1.73, and for composition C it was 1.80.
Using the same total dosage and two scans, the distortion factor was at least halved for each composition. More particularly, the distortion factor for composition A was 1.23, for composition B it was 1.30, and for composition C it was 1.37. Also, in each instance the methyl ethyl ketone extractables were reduced (and the reduction was more than 50% for the slowest curing composition A).
The invention is defined in the claims which follow.