US 4,921,922 AGrant
Production of Tetrafluoroethylene Polymers
Issue Date:1990-05-01
•2 Claims
Abstract
Production of coagulated dispersion grades of PTFE using an aqueous emulsion polymerization process which employs an initiator system comprising disuccinic acid peroxide and ammonium sulphite, the latter being added during the course of the polymerization. The resulting polymer can be fabricated into porous products of improved properties.
Metadata
Assignee
- Imperial Chemical Industries PLC
Inventors
- Terence E. Attwood
- Richard F. Bridges
Application Information
Application Number:US 201209&
Filing Date:1988-06-02
Priority Date:1986-11-26
Art Unit:155
Classifications
IPC:
C08F 1418
Field of Search:
52681;255
Patent Drawings
This patent does not have any drawings.
Description
Example C1
This was a control employing only DSAP (0.72 g; 0.012% on water charged) for the initiator system. The polymerisation was continued to 31% solids content, corresponding to 2695 g TFE having been reacted. The reaction time was 123 minutes, the peak reaction rate was 2.6 mole/litre/hour, and the rate at reaction end was 1.9 moles/litre/hour.
Example 2
In this polymerisation (according to the invention), which was continued to 30% solids content corresponding to 2570 g TFE having been reacted, the initiator system employed was DSAP (0.72 g; 0.012% on water charged) with AMS (50 ppm based on water; 41.7% based on DSAP) being added (after 30 minutes) at 6% solids content, corresponding to 383 g TFE having been reacted (14.9% conversion). The reaction time was 190 minutes, the peak reaction rate was 2.4 moles/litre/hour, and the rate at reaction end was 0.9 moles/litre/hour.
Example C3
In this polymerisation (not according to the invention), which was continued to 30% solids content corresponding to 2570 g TFE having been reacted, the initiator system used was DSAP (0.72 g) with sodium metabisulphite (10 ppm based on water) being added (after 16 minutes) at 2% solids content, corresponding to 122 g TFE having been reacted. A further 10 ppm of sodium metabisulphite was added (after 31 minutes) at 6% solids content, corresponding to 383 g TFE having been reacted, since the first addition showed little effect. The reaction time was 128 minutes, the peak reaction rate was 2.5 moles/litre/hour, and the rate at reaction end was 2.0 moles/litre/hour.
Example C4
In this polymerisation (not according to the invention), the initiator system used was DSAP (0.72 g) with ferrous sulphate (2 ppm based on water) being added (after 28 minutes) at 6% solids content, corresponding to 383 g TFE having been reacted. The reaction time was 68 minutes, the peak reaction rate was 6.2 moles/litre/hour, and the rate at reaction end was 5.3 moles/litre/hour.
Example C5
In this polymerisation (not according to the invention), the initiator system used was DSAP (0.06 g) with hydroquinone (2 ppm based on water) being added (after 48 minutes) at 2% solids content, corresponding to 122 g TFE having been reacted. The reaction time was 167 minutes, the peak reaction rate was 4.2 moles/litre/hour, and the rate at reaction end was 0.8 moles/litre/hour.
The TFE polymers from Examples 1 to 5 were evaluated using the Stretch Test and Differential Scanning Calorimeter (DSC) Test as follows.
Stretch Test 200 g of polymer were sieved through an 8 mesh screen and 43 g Isopar H lubricant (inert hydrocarbon) added. The mix was rolled for 25 minutes, then conditioned for 24 hours at 25.degree. C. The mix was sieved, extruded at 20 mm/min (30.degree. C.) with a reduction ratio of 100:1 through a 2.54 mm die. The extrudate was dried in a vacuum oven for 2 hours at 100.degree. C., then baked for 3 minutes at 190.degree. C. The extrudate was then heated to 300.degree. C. and drawn (6:1) in a tensiometer (Instron) at 17% per second to give a porous product. A 2 cm sample length was used.
DSC Test In a differential scanning calorimeter (Perkin Elmer DSC II), a 10 mg sample of polymer was heated from 280 to 380.degree. C. at 10.degree. C./minute. The sample was cooled to 280.degree. C. at 10.degree. C./minute. and reheated to 380.degree. C. at 10.degree. C./minute. The ratio of reheating and cooling peak heights R/C was measured. This gives an indication of molecular weight; the larger the number, the higher the molecular weight.
The SSG values of the polymers were also determined.
The following results were obtained:
It was thus found that the PTFE made according to invention (Example 2) gave product with the best appearance using the Stretch Test. It also had the highest molecular weight on the balance of the DSC and SSG measurements (highest outright on the DSC Tests; approx. equal highest with Example C5 on SSG measurements).
Claims
We claim:
1. A coagulated dispersion grade tetrafluoroethylene homo- or copolymer produced by a process which comprises emulsion polymerising tetrafluoroethylene, or tetrafluorethylene with one or more comonomers, in an aqueous medium in the presence of a surfactant(s) as emulsifying agent and a water-soluble initiator system comprising disuccinic acid peroxide and ammonium sulphite, the ammonium sulphit- being added to the aqueous reaction medium after the start of polymerisation, namely at a conversion within the range 1 to 95%, and the amount of ammonium sulphite employed being within the range 25 to 300% by weight, based on the weight of the disuccinic acid peroxide used.
2. A coagulated dispersion grade tetrafluoroethylene homo- or copolymer according to claim 1, which is in the form of a fabricated porous product which has been uniaxially or biaxially stretched during its manufacture.