The invention concerns a process for joining together by hot pressing molded parts having a silicon nitride surface at least in the region of the joint, in which process polished surfaces to be joined with or without an interposed silicon layer, are bonded together at pressures of at least 10 MPa and temperatures above 1300.degree. C.
Various processes are known for joining Si.sub.3 N.sub.4 ceramic parts. These can in a general way be subdivided into two groups of processes which respectively operate with and without addition of other (foreign) matter.
In the first group is a joining process in which the bonding of molded parts made of isostatically hot pressed silicon nitride (HPSN) or reaction bonded Si.sub.3 N.sub.4 (RBSN) is intended to be obtained by nitriding an interposed silicon disk. According to another process, the bond between HPSN or RBSN ceramics is produced by hot pressing(HP) or isostatic hot pressing (HIP) with an interposed layer of Si.sub.3 N.sub.4 powder or an interposed RBSN disk. After isostatic hot pressing, bending strength values up to 276 MPa at room temperature are obtained.
In the second group, there are processes using intermediate layers of individual metals, alloys, oxide compounds, glasses, etc. Thus, for example, Si.sub.3 N.sub.4 bodies having a disk interposed between them consisting of W, Mo, Cr or Co are bonded together by pressure welding. The products thus obtained, however, show the formation of cracks in the boundary layer. The joining of the Si.sub.3 N.sub.4 bodies with the help of successive graduated layers of Si.sub.3 N.sub.4 and W powders has seemed more promising: In this case, a faultless bond with shear strengths from 100 to 200 MPa was obtained.
Various solders have been mentioned in the literature for insertion between Si.sub.3 N.sub.4 workpieces to produces a joint. Active solders or brazing compounds made from the elements Ag, Ti, Zr, Be, Cu, etc. have been found useful in this regard. The eutectics thereby formed indeed have good wetting properties, but the temperature stability of such compositions is small, however.
Substantial strength values were successfully reached by means of glasses of the SiO.sub.2 +Al.sub.2 O.sub.3 +Y.sub.2 O.sub.3 or SiO.sub.2 +Al.sub.2 O.sub.3 +MgO compositions. The Si.sub.3 N.sub.4 surface reacted with the glass melts at temperatures around 1600.degree. C. (pressure: 200 KPa; time: 45 minutes). The Si.sub.2 N.sub.2 O thereby formed grew out from the Si.sub.3 N.sub.4 surface into the weld seam. At the same time, the melt diffused along the grain boundaries into the Si.sub.3 N.sub.4. Up to 800.degree. C. a 4-point bending strength (.sigma..sub.4B) of .about.450 MPa was measured. With rise of the temperature, this value grew still further, but at 1000.degree. C. it nevertheless sank to zero.
Si.sub.3 N.sub.4 was bonded in accordance with another process by means of SiO.sub.2 +CaO+TiO.sub.2 glasses. Breaking strength experiments showed, however, that the .sigma. values of the joint seam that was about 20 .mu.m thick did not go above 280 MPa.
These joining processes, whether worked with or without a foreign substance in the region of the joint, are not fully satisfactory, because either no convincingly good bond is obtained or else the nitriding cannot be obtained uniformly over the entire region of the joint, or else a weakening of the boundary layer is to be expected particularly on account of the effect of temperature on strength.
SUMMARY OF THE INVENTION
It is accordingly an object of the invention to provide a process by which a uniformly good bond of the molded parts can be obtained across and beyond the joint region, a bond which is not subject to weakening in the joint seam as a result of the presence of foreign materials.
Briefly, at least on one of the surfaces to be joined a sputtered layer of silicon nitride is applied before hot pressing which has an excess of nitrogen in its composition and then, in hot pressing for joining the parts, measures are taken to provide a complementary nitrogen deficiency in the joint region.
In other words, in accordance with the invention, measures are taken to provide a nitrogen excess in the region of the boundary layers growing together and a nitrogen deficiency in the material itself, so that merely by reactive sorting out and diffusion into each other of the complementary layers, a growing together of the bodies can take place across the boundary layer, by which the seam practically vanishes.
The nitrogen excess is produced by building up an Si.sub.3 N.sub.4+ layer by sputtering of silicon in a regulated nitrogen containing atmosphere. "Sputtering of silicon" is to be understood, in the context of the foregoing description, as also including plasma supported processes in which the silicon is brought forth in the reaction chamber either as such or in the form of a compound.
The corresponding nitrogen deficiency can be formed either by a surface layer consisting only of silicon or likewise by sputtering of an obtainable Si.sub.3 N.sub.4- layer. In particular, these layers or sputtered coatings provided on the finely polished surfaces of the molded bodies are thinner than about 2 .mu.m, and layer thicknesses exceeding the value of the maximum surface roughness of the bodies to be bonded are of minor interest. Thicknesses in the region from 0.1 to 0.3 .mu.m are particularly desired and sought.
The atomic composition of the sputtered layer which is built up by sputtering in nitrogen depends with relatively great sensitivity, on the nitrogen pressure that prevails during the sputtering of the silicon, and, in fact, especially in the deficiency region while an approximate saturation is established in the nitrogen excess region, all of which leads more or less to compositions corresponding to Si.sub.3 N.sub.5.5, so that the building up of these same nitrogen-excess silicon nitride layers seems particularly practical.
It further seems useful to provide immediately on top of such nitrogen-excess layers a deposit of silicon of about half the thickness, so that later when two analogously pretreated molded bodies are joined, a growing together across the location of the joint seam can be obtained by melting together and interpenetrating reaction.
Good results are also obtained, however, by generating a nitrogen-deficiency layer of the composition Si.sub.3 N.sub.2.5 which is complementary to the Si.sub.3 N.sub.5.5. Such a nitrogen deficiency layer can be obtained by sputtering silicon in a correspondingly reduced (rarefied) nitrogen atmosphere.
The formation of such silicon nitride sputtered layers by silicon sputtering is in itself known and the desired production of a nitrogen excess or of a nitrogen deficiency, dependent upon the prevailing nitrogen pressure and the other conditions, such as absolute pressure, spacing between sputtering electrode and substrate, applied voltage, etc., can be determined directly and simply by a preliminary run of the operation. In particular, and by way of example, nitrogen pressures in the region from 10.sup.-3 to 10.sup.-1 mbar are useful and applied voltages between a few hundred volts and durations of sputtering between 10 and 100 minutes.
Further details of experimental information regarding sputtering nitrogenous silicon films are published in our article in Thin Solid Films (1987), pp. 223-233.
Immediately before the application of such sputtered layers, the surfaces to be joined are preferably cleaned by "bombardment" with argon ions ("argon-etched").
The joining procedure is carried out most successfully at temperatures in the region from 1500 to 1750.degree. C. and pressures applied to press the parts together are preferably in the region from 10 to 30 MPa, for application for 20 to 120 minutes or somewhat more in a press which is evacuated and flushed with N.sub.2.
When Si.sub.3 N.sub.4 molded parts of HPSN material are used which have been produced with addition of a small amount of Y.sub.2 O.sub.3, yttrium oxide present in the surface appears to have an effect as an aide to consolidation.
The invention will now be described by way of illustration with reference to an example of performance of the process.
EXAMPLE
Preparation of Samples
Prismatic samples measuring 12.times.12.times.5 mm or 16.3.times.1.3.times.5 mm (both sizes have been used in this example) were polished at their faces which were to be joined (12.times.12 mm or 16.3.times.16.3 mm as the case may be). These samples were of HP quality Si.sub.3 N.sub.4 obtained from the Hertel-International firm in Germany. The polished samples, before the application of layers thereto, were then cleaned in an ultrasonic bath and dried. Immediately before sputtering on of the SiN.sub.x layers, the polished surfaces were etched with Ar.sup.+ ions in situ after having been installed in the sputtering apparatus through vacuum locks. Thin films were applied by reactive sputtering of a silicon target in the presence of N.sub.2. For this purpose a sputtering apparatus with a planar HF magnetron cathode was used (Type Z 400 of the Leybold-Heraeus firm of Germany).
Joining of Samples
For joining together the Si.sub.3 N.sub.4 samples, two varieties of layers were provided to the parts for different joining conditions, as the following table shows.
The sputtered pairs of samples were joined together in a laboratory hot press. During the pressing operation, the Si.sub.3 N.sub.4 samples were located in a graphite guide structure in order to to prevent lateral shifting. For avoiding a chemical reaction between metallic pressing dies and the sample, the contact surfaces were isolated from each other by graphite cylinders or SiC disks. The press chamber was evacuated and flushed with N.sub.2 several times before hot pressing. In each case an N.sub.2 pressure of 40 KPa was established before pressing. The test samples were cut perpendicularly to the joint seam and then were examined with a light microscope as well as with an electron beam microsonde, by which it was established that the joint seam was no longer recognizable.
Although the invention has been described with reference to a particular example, it will be recognized that variations and modifications are possible within the inventive concept.