US 4,853,432 AGrant
Pressure Sensitive Adhesives Containing Light Color, Low Softening Point Hydrocarbon Resins
Issue Date:1989-08-01
•10 Claims
Abstract
An adhesive comprising a copolymer and an optionally hydrogenated light color petroleum hydrocarbon resin including an aromatic hydrocarbon component useful for tackifying block copolymers is described which has a softening point of about 0.degree. C. to about 40.degree. C., a number average molecular weight (Mn) of from 350 to 600 and a molecular weight distribution (Mw/Mn) of from 1:1 to about 2.0.
Metadata
Assignee
- Exxon Chemical Patents Inc.
Inventor
- Mary E. Ahner
Application Information
Application Number:US 0685909
Filing Date:1987-06-30
Priority Date:1986-02-18
Art Unit:151
Classifications
IPC:
C08L21700C08L 9304
Field of Search:
526525524290232;236;237274;575;524;525;526
Patent Drawings
This patent does not have any drawings.
Description
The resins of this invention can be readily prepared from the foregoing description and the following examples. Those skilled in preparing adhesives from petroleum hydrocarbon resins will be able to incorporate same with copolymers. Accordingly, this invention is further described by the following examples which are offered by way of explanation and for the purposes of guiding those skilled in the art to the practice of this invention and the broadening of its usefulness and not for purposes of limitation thereof and it should not be so construed.
EXAMPLES 1-4
The liquid resins of Examples 1-4 were polymerized batchwise using aluminum chloride catalyst in a nitrogen atmosphere at about 12 psig (0.84 Kg/cm.sup.2). The aluminum chloride catalyst (having particle size between 5 and about 200 mesh) is added in anhydrous form. In these polymerizations, 400 grams of feed blend, in proportions indicated in Table 1, were pumped into a closed, stirred reactor containing catalyst, over a thirty minute period of time and then left in contact with the catalyst for an additional thirty minutes with stirring. A 400 gram 1:3 solution of isopropanol:water was added to the reaction mixture to quench the catalyst and the polymerizate was water washed two to three additional times with the aqueous phase being separated after each wash.
The polymerizate was finished by heating to 250.degree. C. in a nitrogen atmosphere to remove unreacted material. The polymerizate was then steam stripped at 250.degree. C. to produce the finished resin.
In Examples 1-4, the xylenes, styrene, p-methylstyrene, mixed methyl styrenes and alpha-methylstyrene components were of at least 96% purity. The compositions of the heat soaked piperylene concentrate and isoamylene concentrate used are shown below:
These examples show the influence of aromatic olefin structure on resin properties. Resin properties are shown in Table 1 below:
The ring and ball softening points of the resins were determined using a modified ASTM E-28 procedure. The softening point was measured in a 50/50 ethylene glycol/water solution. The rings were kept in a -25.degree. to -30.degree. C. environment until the ethylene glycol/water solution was cooled to that temperature range. The ring and ball softening point apparatus was assembled and heated at 5.degree. C./min. The softening point temperature was then read according to the ASTM E-28 procedure.
EXAMPLES 5-13
In Examples 5-13, a styrene concentrate fraction of steam cracked naphtha boiling within the range of from 80.degree. C. to 190.degree. C. was used with the isoamylene and piperylene concentrate to prepare resins in the manner described in Examples 1-4 about in proportions as set forth in Table 3. The compositions of the styrene concentrates are shown in Table 2 below:
These resins were polymerized and finished, and the softening points were determined using the same procedures discussed in Examples 1-4. These examples show the effect of varying feed blend ratios on resin properties. Note the high color and softening points of certain resins derived from the styrene concentrates.
Examples 10, 12 and 13 show the effect of styrene concentrate composition on resin properties.
EXAMPLES 14-20
In Examples 14-20, a mixed C.sub.6 monoolefin stream prepared from the dimerization of propylene was used in place of isoamylene concentrate in resins produced as described in Examples 1-4 above. Typical compositions of the C.sub.6 olefin stream and the piperylene concentrate used in these examples follow:
In these Examples, pure styrene and alpha-methyl-styrene monomers were used as the vinyl aromatic hydrocarbon stream resulting in resins having an aromatic content from about 10 weight percent to about 60 weight percent and a Gardner color of about 1. The feedstock composition and resin properties are shown in Table 4 below. These resins are particularly useful to prepare adhesives in the practice of this invention.
EXAMPLES 21-23
In These examples, the mixed C.sub.6 monoolefin stream prepared from the dimerization of propylene was used again in the monomer described for the examples above. However, in Example 21 no piperylene was used; in Example 22 an ethyl aluminum dichloride catalyst was used; and in Example 23 a BF.sub.3 O(CH.sub.2 CH.sub.3).sub.2 (etherate) catalyst was used for Friedel Crafts polymerization. The feedstock composition and resin properties are shown in Table 4A below.
In Examples 24-26, a heart cut distillate (80.degree. C. to 260.degree. C.) derived from steam cracked naphtha was used in place of the pure vinyl aromatic monomers in resins produced as described in Examples 1-4 above. A typical composition of this heart cut distillate is shown below.
The feedstock compositions and resin properties are shown in Table 5 below:
EXAMPLES 27 and 28
In the manner described in Examples 1-4, Examples 27 and 28 demonstrate the use of diisobutene and an isoamylene concentrate to prepare resins within the scope of the invention. The resin of Example 27 was stripped excessively, resulting in a softening point of 41.degree. C. If excessive stripping had not occurred, the softening point would have been 40.degree. C. or less with a Gardner color of about 2 also resulting. The results of these experiments are shown in Table 6:
The low softening point liquid resins described above are all applicable in the practice of the instant invention to make adhesives when combined with a copolymer. The copolymers useful for the practice of this invention are generally known as, for example, styrene/isoprene/styrene (SIS), polyethylene vinyl acetate (EVA) (from about 25% to about 45% by weight vinyl acetate), styrene/butadiene/styrene (SBS) and styrene/ethylene/butylene/styrene (SEBS), and the like. Of particular interest are the styrene/butadiene copolyers which are classically more difficult to tackify than other polymers using a resin and often require not only a tackifier but an oil to act as a plasticizer thus giving rise to the problem of "bleed" and/or "creep" when the adhesive is applied to a paper or polymer substrate. When the need is for a light color, essentially water white resin, previously only resins prepared from nonaromatic materials were available since aromaticity had heretofore imparted color to the resin which was unacceptable for certain applications, including premium packaging and disposable diapers. The presence of an oil in the adhesive composition has other detrimental effects such as unacceptable creep and bond release along a polyethylene film, particularly in a case where disposable diapers are involved. Thus, the resins described above, particularly those of Examples 14-20 which can be used with styrene/butadiene polymers in a binary system, i.e., by eliminating the plasticizer, are particularly useful.
Well known styrene/butadiene copolymers useful in the practice of this invention are those sold by shell under the "Kraton" trademark and by Firestone under the "Stereon" trademark. Both of these are styrene/butadiene copolymers which form particularly attractive adhesives when used in combination with the above-identified resins, particularly the very low color resins of Examples 14-20 having a softening point of around 20.degree. C. The "Stereon" copolymer grade 840A is a copolymer containing 42% styrene. In formulating the adhesive, the liquid resin is present in amounts from 20% to 80% by weight with the copolymer present in, correspondingly, 80% to 20%. The preferred adhesive would contain from about 30% to about 70% by weight of the resins with from about 35% to about 50% by weight in the adhesive being especially preferred. In binary adhesives, the copolymer will be present in corresponding amounts. However, other components may be present. Optionally, a resin having a higher softening point, from about 80.degree. C. to about 120 .degree. C., may be used as an additional component of the adhesive composition. While the preferred adhesive is a binary system comprising two reactants, the copolymer and the light color resins described herein, such binary system may still include such nonreactive ingredients as fillers, inhibitors, and the like. Representative of fillers would be, for example, calcium carbonate, titanium oxides, finely divided clays, talc and the like.
Once blended using methods and techniques well known to those skilled in the art, the adhesive would be coated on a substrate such as "Mylar" film (Dupont Company) or "Endura" film (Akrosil). The adhesive is then evaluated in terms of those parameters important to adhesives such as rolling ball tack, polyken tack, peel strength, holding power and aged retention of these properties.
The adhesive compositions of the present invention may be applied to a substrate and, if solvent coated, dried using conventional procedures. The substrate used depends upon the anticipated use, but it is usually relatively thin material, usually no greater than about 3.2 mm in thickness, and in the manufacture of tapes and labels, the substrate is a relatively thin sheet material. The sheet material may be a polymeric material which is flexible at about room temperature. The sheet material may be a homo-polymer of an ethylenically unsaturated monomer such as ethylene, propylene or vinyl chloride, or be polyester, polyacetate or polyamide provided it has sufficient flexibility for the desired end use. Alternatively, the substrate may be made from cellulosic or reconstructed cellulosic material such as rayon. The substrate need not be a sheet material but may be composed of fibers which may be woven, or nonwoven as in the case in paper. Woven substrates may be made from cellulosic material, such as cotton or from fibers of any of the above mentioned polymers.
The composition is applied to the substrate using conventional coating techniques such as roller coaters, blade coaters, meyer rods or air coaters. The coated substrate can be dried usually by passing it through a heating tunnel or oven through which may be circulating hot air or the tunnel or oven may contain infrared lamps to dry the coated substrate. The drying time will be a function of a number of factors such as the heat capacity of the substrate, the type of heating, the oven temperature, air velocities (if circulating air is used) and the rate off passage of the substrate through the heater.
The substrate should be coated with sufficient composition to provide a dry coat weight from about 16 to about 57 g/m.sup.3. Generally in the manufacture of tapes using a continuous sheet polymeric substrate, a dry coat weight of about 15-30 g/m.sup.2 is used. In the manufacture of labels, a dry coat weight from about 15 to 30 g/m.sup.2 is usually used. In the manufacture of masking tape, a dry coat weight from about 35 to about 65 g/m.sup.2 is usually used.
After drying, the coated substrate is cut to the required dimension. In the manufacture of tape, the substrate is cut into strips and rolled to provide a finished product. The substrate may also be cut into shaped items to provide labels or medicinal tapes.
One particularly attractive use for the pressure sensitive adhesives of the present invention is in diaper tabs for disposable diapers, particularly repositional tabs which employ a "Mylar" polymer substrate coated as stated above with 1.5 mil adhesive as shown in Table 7 below.
The mechanical preparation of the adhesives of this invention are well known to those skilled in the art. In addition to the components which make up the adhesives of this invention, i.e., the copolymers and the low softening, light color resin described above, other materials, well known to those skilled in the art may be added without departing from the invention such as, for example, fillers or resins having higher melting points such as, for example, from about 80.degree. C. to about 120.degree. C. in order to impart additional strength to the resulting pressure sensitive adhesive. In some applications, it may be desirable to add up to about 60 weight percent of such "hard" resin such as that described in U.S. Pat. No. 4,514,554 for example, the disclosure of which is incorporated herein by reference, and U.S. Pat. No. 4,391,961. Both provide often desirable modifications of the pressure sensitive adhesive of this invention.
Preferred adhesives are made with a styrene/butadiene copolymer having from about 40% to about 50% styrene. In use, the adhesives are applied to a polyacetate or cellulose backing in a thickness of from 0.7 to 1.5 mil. To illustrate the present invention, adhesives were made by mixing a styrene/butadiene copolymer having 42% styrene polymer ("Stereon" Resins from Firestone) with resins similar to, and prepared in the same manner as, those of Examples 16 and 18 and commercially available resins useful to produce adhesives with such styrene/butadiene copolymer. The characteristics of the liquid resins compared are set forth in Table 8.
These resins as shown are used in preparing a repositional diaper tab in varying proportions of resin to copolymer in the manner of mixing well known to those skilled in the art. The adhesive was applied in the amount of 1.5 mil drawdown on 0.005 g/cm.sup.2 "Mylar" polyacetate film backing. The test results are as shown in Table 9 and Table 10.
To further demonstrate the advantages of this invention, a pressure sensitive adhesive is described below using the above described liquid resin, the styrene/butadiene copolymer, and a commercially available inhibitor. The 20.degree. C. softening point liquid resin is similar to the one described in Examples 16 and 18 with the properties as shown in Table 8.
As seen from the foregoing, the pressure sensitive adhesive of the present invention provides considerable advantage over other pressure sensitive adhesives made with available liquid resin.
EXAMPLE 29
Hydrogenation of the resins of the adhesive compositions of the invention results in a color improvement. A resin very much like that of Example 24 and Table 5 was hydrogenated by dissolution of the resin in an inert, predominantly saturated hydrocarbon solvent (Varsol) at 30 wt. % concentration and passing the solution over a sulfided nickel./tungsten/alumina catalyst. The flow rate was 1.5 VVH, hydrogenation pressure 3000 psi and inlet temperature 270 degrees C. The hydrogenated solution was stripped to give a 28.3% yield of product with a color of 28 Saybolt (measured as 10% solution in toluene; water white resin is 30 Saybolt) and softening point of 19 degrees C. The GPC molecular weight was indicated to be the same as for the resin of Example 24 both before and after hydrogenation. The vinyl aromatic content dropped slightly to about 22%. The hydrogenated resin has proven to be an excellent water white tackifier in various adhesive formulations as described above.
Other suitable catalysts for hydrogenation include nickel and palladium based catalysts preferably supplied or alumina or similar material. Hydrogenation temperatures and pressures can be much lower than as given in the example, or higher as needed depending on the catalyst.
The foregoing disclosure and description of the invention are illustrative and explanatory thereof, and various changes in the components, parameters and proportions, as well as in the details of the illustrated examples, may be made without departing from the spirit and scope of the claimed invention.
Claims
I claim:
1. An adhesive composition comprising from about 20% to about 80% by weight of a copolymer and, correspondingly, from about 80% to about 20% by weight of a tackifying hydrocarbon resin having a softening point of from 0.degree. C. to about 40.degree. C., a number average molecular weight of from about 100 to about 600, and a Gardner color less than about 7 prepared by the Friedel Crafts polymerization of a hydrocarbon feed comprising: (a) from about 5% to about 75% by weight of C.sub.8 to C.sub.10 vinyl aromatic hydrocarbon stream; (b) up to about 35% by weight of a piperlene concentrate; and (c) from about 25% to about 70% by weight of a C.sub.4 to C.sub.8 monoolefin chain transfer agent of the formula RR'C.dbd.R"R'" where R and R' are C.sub.1 to C.sub.5 alkyl, and R" and R'" are independently H or C.sub.1 to C.sub.4 alkyl group, wherein said copolymer and said tackifying hydrocarbon resin are compatible.
2. An adhesive according to claim 1 wherein the hydrocarbon resin is prepared by aluminum chloride catalyzed polymerization.
3. An adhesive according to claim 1 wherein the adhesive comprises from about 35% to about 50% by weight of the hydrocarbon resin and said copolymer is a styrene/butadiene copolymer.
4. An adhesive according to claim 1 which also comprises up to about 60 wt% of an additional resin having a softening point of from about 80.degree. C. to about 120.degree. C.
5. An adhesive according to claim 4 wherein said additional resin is aliphatic, aliphatic/aromatic, terpenic, terpenic/aliphatic, terpenic/aromatic, rosin ester, or a hydrogenated product thereof.
6. An adhesive according to claim 1 which also includes up to about 50% by weight of an inert filler.
7. An adhesive composition according to claim 1 wherein the hydrocarbon resin is hydrogenated.
8. An adhesive composition comprising from about 50% to about 65% by weight of styrene/butadiene copolymer and, correspondingly, from about 50% to about 35% by weight of a petroleum hydrocarbon resin having a softening point of from 10.degree. C. to about 30.degree. C., a Gardner color of 3 or less and a molecular weight distribution of from about 1.1 to about 1.3 with number average molecular weight of from about 100 to about 600; said resin being a Freidel Crafts catalyzed resin from a reaction mixture comprising: (a) from about 5 to about 35 parts by weight of alpha-methyl styrene, styrene or mixtures thereof; (b) up to about 26 parts by weight of a heat soaked piperlene concentrate; and (c) from about 25 to about 70 parts by weight of a mixed C.sub.6 monoolefin stream prepared from the dimerization of propylene.
9. The adhesive composition of claim 8 wherein component (a) of the reaction mixture from which the resin is formed is a mixture of substantially pure styrene and alpha-methyl styrene monomers.
10. The adhesive composition of claim 8 wherein the hydrocarbon resin is hydrogenated.