The invention will now be described, by way of example, with reference to the accompanying diagrammatic drawing in which the single FIGURE shows a sectional side elevation of the housing of a high temperature rechargeable electrochemical cell in accordance with the present invention.
In the drawing the cell housing is generally designated by reference numeral 10 and is shown broken midway along its length, typically having an outside diameter of about 50-60 mm and a length of about 30-60 cm. The housing shown is for a cell having a molten sodium anode material, a sodium aluminum chloride liquid electrolyte and an active cathode substance which in its discharged state comprises an electrolyte-permeable porous matrix containing FeCl.sub.2, NiCl.sub.2 or FeCl.sub.2 /NiCl.sub.2 dispersed therein and saturated with said electrolyte, the matrix having sufficient finely divided NaC1 dispersed therein to ensure that, in all states of charge of the cathode substance, the electrolyte is an equimolar mix of NaCl and Al Cl.sub.3, i.e. NaAl Cl.sub.4.
The cell housing 10 comprises a mild steel outer casing 12 having a base in the form of a rim 13 for supporting it in an operative upright attitude on a horizontal support surface (not shown). The casing 12 is attached by welding to a mild steel casing seat 14 at the top of the casing 12. The seat 14 is closed off by an annular stainless steel or aluminum top casing cap 16 welded thereto. The cap 16 has a stainless steel or aluminum, as the case may be, cell terminal post 18 welded thereto. An open-ended beta"-alumina separator tube 20 is located concentrically within the casing 12, the upper open end of the tube 20 being glass welded to an alpha alumina ring 22 which ring seats with a sliding fit at 24 against an inner curved surface provided therefor on the seat 14.
The tube 20 is closed off by a mild steel closure member 26. This closure member 26 clamps the ring 22 against a shoulder 28 on the seat 14 and the closure member 26 is in turn clamped in position by the cap 16. The closure member 26 has an upstanding central socket 30 therethrough, within which is welded a stainless steel or aluminum tubular spigot 32. This spigot is closed off by a stainless steel or aluminum panel 34 which carries an upwardly projecting stainless steel or aluminum cell terminal post 36. The lower end of the spigot 32 projects below the level of member 26, and has a radially outwardly projecting circumferential flange 38 to which a mild steel inner tube 40 is welded. The tube 40 has a nickel mesh 42 wrapped tightly around its outer surface.
The member 26 is sealed to the ring 22 by a nickel O-ring seal 44 located in a circumferential groove 46 in the lower face of the member 26, and the ring 22 is in turn sealed to the seat 14 by a nickel O-ring 48 located in a rebate defined by an annular shoulder 50 in the seat 14 adjacent the shoulder 28. The cap 16 is electronically insulated from the member 26 by an annular mica disc 52, and the member 26 is electronically insulated from the seat 14 by a mica ring 54. The nickel O-ring 44 seats in the groove 46 on the member 26 via an annular grafoil (graphite) disc 56 and on the ring 22 via an annular aluminum disc 58, the O-ring 48 similarly seating on the shoulder 50 via an annular grafoil disc 60 and on the ring 22 via an annular aluminum disc 62.
A mild steel inner casing 64, welded to the casing 12 and seat 14, is located concentrically around the tube 20 and within the casing 12, separated respectively therefrom by annular spaces. The lower end of the casing 64 is closed by a panel 66 of aluminum having a central opening 68 therethrough, the panel 66 resting on a radially inwardly projecting circumferential flange 70 at the lower end of the casing 64. The opening 68 functions to restrict flow between the annular spaces, e.g. in the event of cell damage. A mild steel floor panel 72 is welded to and closes off the lower end of the casing 12.
The socket 30 projects upwardly through the central opening of the cap 16 and, alongside said socket, there is a bleed outlet or opening provided by a mild steel tube 74 welded into a bore in the member 26. The tube 74 has an internally tapped outer end provided with a closure screw 76 and a gold sealing ring 78. A bleed outlet or opening through the seat 14 is provided by a tapped passage 80 through the seat 14 immediately below the shoulder 50. This passage 80 has a tapped outer end provided with closure screw 82 and is provided with an aluminum sealing ring 84. The passage 80 leads into the top of an annular space between the tube 20 and seat 14, which forms an upward extension of the annular space between the tube 20 and casing 64.
The housing 10 is intended to be for a cell of the so-called inside-cathode type, so that the porous cathode matrix (not shown) will be formed on the outer surface of the tube 40, the mesh 42 being embedded in this matrix and the mesh 42 and tube 40 acting as the cathode current collector. The casings 12 and 64 will in turn act as the anode current collector.
In this regard it will be noted that the tube 20 divides the housing 10 into an inside cylindrical cathode compartment, inside the tube 20, and an outside annular anode compartment, between the tube 20 and the casing 12. The tube 40 in turn divides the cathode compartment into a gas chamber defined by the interior of the tube 40 and of the spigot 32, and a cathode chamber defined by the interior of the tube 20 outside the tube 40; and the casing 64 divides the anode compartment into a gas chamber between said casing 64 and the casing 12, and an anode chamber between said casing 64 and the tube 20.
In use, to assemble the cell, the cathode matrix is conveniently vacuum impregnated with liquid electrolyte in situ, via the tube 74, or it can be pre-impregnated externally before loading into the housing. The interior of the tube 20 can then be filled with an inert gas such as argon or nitrogen and then charged with molten liquid electrolyte. Preferably the cathode will be in an overdischarged state and sufficient electrolyte will be fed into the tube 20 to fill the tube 20 outside the tube 40 and partly fill the tube 40 (the housing 10 being in its upright operative condition or attitude as shown in the drawing), the gas in the tube 40 being under pressure and the capacity or volume of the active cathode substance and electrolyte being sufficient so that when the cell is fully charged there is still some electrolyte in the lower end of the tube 40. Instead, liquid electrolyte can be introduced into the tube 20 in particulate solid form to fill the tube 20 outside the tube 40 and partly fill the tube 40, after which it is melted in situ when the cell is raised to its operating temperature. This will automatically pressurize the inert gas inside the tube 40 and any inert gas outside the tube 40 can be bled from the tube 20 via the tube 74 when the cell has reached its operating temperature.
The housing 12 outside the tube 20 can be filled with inert gas via the tube 80 and a starting amount of particulate or solid sodium charged into the casing 12 via the tube 80, sufficient, when molten, to connect the lower end of the tube 20 electronically with the casing 64 and/or panel 66. Instead, a small graphite felt or metal gauze (not shown) can be located in the anode compartment, e.g. between and electronically interconnecting the tube 20 and panel 66.
If the cell is taken, at its operating temperature, from its overdischarged state to its discharged state, sodium ions will move from the liquid electrolyte into the internal crystal structure of the separator tube 20 and sodium metal will pass from the outside surface of said tube 20 into the anode compartment. When the discharged state is reached inert gas in the space between the tube 20 and the casing 64 can, if desired, be bled from this space via the passage 80, after which the tube is closed. The capacity of the cathode will be selected, together with the volumes of the spaces respectively between the casing 12 and casing 64 and between the casing 64 and tube 20, so that when the cell is in its discharged state there is enough sodium in the anode compartment completely to fill the space between the tube 20 and casing 64, and partly to fill the space between the casing 64 and casing 12, the inert gas remaining between the casings 12 and 64 being under pressure. Likewise, the volume of the cathode and the electrolyte used will be selected so that when the cell is fully charged the tube 20 outside the tube 40 will still be completely full of electrolyte and the tube 40 will contain some electrolyte and inert gas under pressure.
After the initial bleeding of the anode chamber has taken place, the cell will be charged up to its charged state, more sodium passing through the tube 20 from the cathode compartment into the anode compartment, so that the level of electrolyte will drop in the cathode gas chamber formed by the tube 40, and the level of sodium will rise in the anode gas chamber between the casings 12 and 64. When the cell is fully charged, the anode chamber may again optionally be bled via the passage 80.
During the next discharge cycle of the cell, sodium will move through the separator tube 20 from the anode compartment into the cathode compartment. The level of sodium in the anode gas chamber between the casings 12 and 64 will drop while the sodium in the anode chamber between the tube 20 and casing 64 will remain at its full level, held there by inert gas pressure in the anode gas chamber. As sodium in ionic form enters the cathode chamber, liquid electrolyte level rises in the tube 80 and inert gas in the cathode gas chamber formed by the tube 40 and spigot 33 is pressurized. At the end of this discharge cycle any gas in the tube 20 outside the tube 40 is bled via the tube 74, electrolyte rising in the tube 20 outside the tube 40 under the influence of gas pressure in the tube 40 and spigot 32. Further gas bleedings via passage 80 and tube 74 can take place after subsequent charge and discharge cycles respectively, if desired.
An advantage of the invention is that a cell is provided wherein it is ensured that all states of charge and discharge, the surface of the separator exposed to the anode compartment and the surface of the separator exposed to the cathode compartment are both at all times fully wetted respectively by liquid sodium and liquid electrolyte. A further specific advantage, when the cathode is loaded in its overdischarged state, i.e. when it is an iron, nickel or iron/nickel matrix containing an excess of NaCl dispersed therein and the liquid electrolyte contains Al, e.g. in particulate form therein, is that the cell can be assembled without any necessity for handling metallic sodium, the cell constituents, particularly if the cathode is loaded cold and pre-impregnated with the electrolyte and the liquid electrolyte is loaded cold in particulate form, being entirely safe to handle. It is also unnecessary, as inert gas is used and the cathode matrix is pre-impregnated with liquid electrolyte externally, at any stage to evacuate the cell during loading.
Finally, it should be noted that the method described above for loading an inside-cathode cell is equally applicabble to an outside-cathode cell; wicking of the sodium is not needed as inert gas pressure in the anode gas chamber keeps sodium level up to the desired height at all times; and it should also be noted that in principle non-return valves can replace the closure screws 76 and 82.
In a refinement of the invention each electrode compartment is preferably pressurized to substantially above atmospheric pressure, e.g. to a pressure of about 3-6 atmospheres. This can be effected by loading a suitable amount of sodium azide into each electrode chamber, and heating the cell to a temperature, above 320.degree. C. sufficient to decompose the sodium azide. Sodium azide is NaN.sub.3 and decomposes in the temperature range 280.degree.-320.degree. C. according to the formula ##STR1##
The sodium azide may be introduced into the cell wrapped in a suitable metal foil (eg nickel foil) compatible with the cell environment, in the form of a tablet containing inert binder, or the like. It is preferably located in position in each of the gas chambers above the maximum anticipated liquid levels in said gas chambers, e.g. as shown at 86 and 88 in the drawing. The sodium azide may be loaded into the cell at any convenient stage of loading the cell, e.g. before adding liquid electrolyte to the cathode compartment and before adding any sodium to the anode compartment.
When the cell is heated to its operating temperature, it can be heated to a temperature, e.g. slightly above 320.degree. C., sufficient to decompose the sodium azide. This causes release of nitrogen (inert gas) which will pressurise the electrode compartments to a substantially greater degree than mere heating to the normal operating temperature.
Loading the cell will otherwise be substantially as described above and the electrode chambers will be bled as described, although gas at a higher pressure will be released. Sufficient sodium azide will be loaded to obtain the desired pressures, and the sodium produced by the decomposition will cause no problems. The elevated pressures will ensure that both sides of the separator are fully wetted at all times by forcing liquid under pressure into the electrode chambers.