Background of the Invention
This invention relates to a low modulus damping film, and more particularly to a coil winding support for superconducting generator applications.
Superconducting generator applications require fast spin-up and rapid excitation. This start-up requirement necessitates a high field, high current advanced conductor such as Nb.sub.3 Sn, and a winding design which offers uniform mechanical support to prevent conductor motion. A fully epoxy impregnated winding of multistranded Nb.sub.3 Sn conductor satisfies both of these requirements. U.S. Pat. No. 3,991,333 shows a typical superconductive generator of this type, showing the use of Mylar inserted between each winding and its adjacent supports, to provide electrical insulation for the windings.
The epoxy-impregnated winding, however, must be rigidly supported with additional precompression to accommodate the centrifugal forces. As a result the coil winding support for a satisfactory design must be intimately interfaced with the impregnated winding. High shear strains can thus be transferred to the coil module which may facture and degrade the winding operation.
U.S. Pat. No. 4,037,312 to Deis discloses an insulating material of a layer of phenolic modified polyvinyl formal covered or coated with a bonding material of epoxy applied to a wires of a cable in a superconductive rotor coil. U.S. Pat. Nos. 3,662,461 to Lake, 3,705372 to Gotal and 4,467,303 to Laskaris are also of interest.
Summary of the Invention
An object of the invention is to provide a low modulus interface material which will be able to absorb shear strain due to a combined compression-tension load due to differential thermal contraction.
The invention relates to a low modulus damping film which occupies the interface area between the outer winding surfaces and the winding support of an epoxy impregnated Nb.sub.3 Sn superconductor in a generator. The polycarbonate Makrofol KG (Mobay chemical) 16 disclosed as the preferred damping or interface film. An adhesive such as the polyurethane Bostik 7070 is used for affixing the film to the winding surface.
Brief Description of the Drawing
FIG. 1 is a perspective view, and FIG. 2 is a cross section view taken along lines 2--2 of FIG. 1, of a fully impregnated Nb.sub.3 Sn coil module to which the Makrofol (polycarbonate) film was satisfactorily applied.
Detailed Description
The low modulus damping film occupies the interface area between the outer winding surfaces and the winding support. This film must be able to absorb shear strain due to a combined compression-tension load due to differential thermal contraction, magnetic, and centrifugal forces. Pertinent mechanical and physical property information on thin film polymers were identified in two references, (1) Muller, A. C., "Properties of Plastic Tapes for Cryogenic Power Cable Insulation", 1978 ICMC Meeting, July 10-11, Munich, Germany; and (2) Jelinek, F. and Muller, A. "Study of the Dimensional Behavior of Various Thin-Film Polymers in the Temperature Range 4.2.degree. K. to 300.degree. K.", Advances in Cryogenic Eng. 22, 312 (1977). Two materials were selected as suitable, Mylar and Polycarbonate. Mylar or polyethylene terephthalate is a high molecular weight polyester with a relatively high melting point. The polycarbonate is a non-polar, linear polyester of carbonic acid derived from bisphenol A.
The significant properties of these two polymers are shown in Table I. The Mylar film is available from DuPont in various thicknesses. The specific polycarbonate is identified as Makrofol KG and is available from the Mobay Chemical Co. It is a semi-crystalline film biaxially oriented. The pertinent dielectric and tensile properties of these materials at 293.degree. K. and 4.degree. K. are shown in Table II. The data shows that both of these materials maintain high elongation at 4.degree. K. In the Muller paper (reference 1) mention is made that certain polymeric thin films fracture when cooled to 6.degree. to 10.degree. K., while other materials resist thermal fracture consistently. Those materials which fracture readily have elongations only slightly larger than their contractions. Those materials having elongations greater by a factor of ten or more always resist fracture. Table II shows that for Mylar this ratio is 10 and for the Makrofol KG it is 22.
In view of the superior elongation properties of the Makrofol KG (polycarbonate) this material should be more effective as a damping interface. The recent superconducting rotor dynamics program funded by the Air Force selected this material for the coil winding interface. A polyurethane adhesive (Bostik 7070) was used for affixing the film to the winding surface. The adhesive was applied by diluting the Bostik with methylene chloride and spraying the diluted mixture.
Thermal cycling by rapid cooling in liquid nitrogen did not show any crazing, cracking or lifting of the film. A low modulus damping film Makrofol KG-polycarbonate has been identified and experimentally evaluated as an interface material for superconducting coils.
The drawing shows a fully impregnated Nb.sub.3 Sn coil module to which the Makrofol (polycarbonate) film was satisfactorily applied. The coil 10 has the polymer film 12 applied to the outer surface, as well as the upper and lower surfaces, as shown. The polymer film is affixed to the winding surface with the adhesive (not shown). In the perspective view of FIG. 1, the winding spiral shows through the thin polymer film.
It is understood that certain modifications to the invention as described may be made, as might occur to one with skill in the field of the invention, within the scope of the appended claims. Therefore, all embodiments contemplated hereunder which achieve the objects of the present invention have not been shown in complete detail. Other embodiments may be developed without departing from the scope of the appended claims.