Brief Description of the Drawings
FIG. 1 is a block diagram depiction of the method of fabricating substrates in accordance with the present invention;
FIG. 2 is an exploded perspective view of a portion of an illustrative substrate;
FIG. 3 is a perspective view illustrating the substrate of FIG. 2 with microelectronic conductors and circuit components received thereon; and
FIG. 4 is a partial view in cross section along lines 44 of FIG. 3.
Corresponding reference characters indicate corresponding parts throughout the several views of the drawing.
The exemplifications set out herein illustrate a preferred embodiment of the invention in one form, and such exemplifications are not to be construed as limiting the scope of the disclosure or the scope of the invention in any manner.
Description of the Preferred Embodiment
Referring first to the process depiction of FIG. 1 and the exploded perspective view of FIG. 2, sheets of wire cloth, such as an about 100 mesh copper screen having a thickness of about 10 to 12 mils and porcelain green sheets, for example, of the porcelain tape variety described in the above mentioned copending application, are provided from supply sources 11 and 13 respectively with the wire cloth sheets illustrated at 15 and 17 in FIG. 2 while the porcelain green sheets are illustrated at 19 and 21. The sheets are interleaved or superposed in layers at process stage 23. In one preferred form, every pair of wire cloth sheets is separated by at least one porcelain green sheet and most typically, by exactly one porcelain green sheet, while the upper and lower outermost porcelain green sheet layers are formed as three adjacent pieces of porcelain tape. This thicker outer layer aids in reducing any wrinkles or corrugations which might be induced due to the irregularities in the woven copper screen. Five screen layers with four intermediate separating porcelain tape layers and an additional three layers of tape at the outer surfaces has been found suitable.
Once the layers are appropriately interleaved, those interleaved sheets are subjected to pressure at process stage 25 so as to compress the interleaved sheets against one another, thereby forming a laminated composite substrate form still in a green state. This pressure may be accompanied by an elevation in temperature, for example, to around 200.degree. F. (about 90.degree. C.) with the pressure lamination occuring at around 4000 to 5000 pounds per square inch and for a time interval of, say, 3 to 5 minutes. Under such pressure the green sheets or porcelain tape tends to form about individual strands of the screen somewhat as illustrated in FIG. 4.
Subsequent to the pressure lamination the composite substrate, still in its green state, is kiln fired at 27, which again for exemplary purposes may be performed for about a six minute interval with the substrate temperature reaching a peak of around 700.degree. C. Subsequent to such firing, the surface which is now a glazed porcelain surface, may be too irregular for some microelectronic circuit purposes, in which case an optional pressure flattening of the kiln fired sheets as illustrated at 29, may be performed. Such pressure flattening could be by compression between a pair of flat plates and at an elevated temperature of, say around 670.degree. C. The thus formed substrate, either with or without the optional pressure flattening 29, may then undergo subsequent processing 31 of conventional type, such as the screening of thick film paints onto the glazed porcelain tape surface 33.
Referring now to FIGS. 2 and 4 the substrate includes three sheets of porcelain tape 35, 37 and 39 followed by a wire cloth sheet 15 and then alternating porcelain tape and wire cloth sheets, such as 19, 17 and 21, continuing through a sequence of five wire cloth sheets and terminating at the bottom of the substrate with another three consecutive layers of porcelain tape.
The step of subsequently processing as depicted at 31 in FIG. 1, may include the painting or screening of thick film conductors, such as 41 and 43, to adhere to the surface of the substrate by conventional techniques and, again by conventional techniques, a plurality of surface mounted devices, such as 45 and 47, may be affixed to the porcelain substrate as by soldering to the thick film conductors. The good thermal conductivity of the copper allows these components, such as 45 and 47, to be mounted on the porcelain substrate in a high density manner while still adequately cooling the components. Components 45 and 47 as well as the thick film conductors 41 and 43 as illustrated in FIGS. 3 and 4 are, of course, only for illustrative purposes since the substrate 49 is, in a sense, a general purpose substrate and may be used for either thick or thin film purposes or other microelectronic application as desired.
The composite substrate, as thus far described, is particularly useful when its linear coefficient of thermal expansion is matched to the coefficient of surface mounted devices, such as resistors or capacitors, to be mounted on the substrate, since under the circumstances even though the substrate may expand due to heating, the surface mounted devices also expand reducing the likelihood of damage to components or connections due to that thermal expansion. Many of the surface mounted devices contemplated for use with the present substrate are alumina, which has a linear coefficient of about 60 inches per inch per degree centigrade and the substrates manufactured according to the techniques of the present invention generally lie withing the range of 50 to 120 inches per inch per degree centigrade with that coefficient being determined mostly by the glass employed in the tape composition.
In the aforementioned copending application, two specific examples of tape composition by weight, one for steel substrates and another for aluminum substrates, were disclosed. A presently preferred tape composition for use in the present invention is as follows:
500 g: Glass
116.7 g: Acryloid B7
45.0 g: MEK
100.0 g: Toluene
62.5 g: Acetone
12.0 g: Sanicizer 261
2.2 g: DC#3
The glass material in this typical tape composition is ELPOR 2010 available from Ferro Corporation, Cleveland, Ohio, while the remaining constituents are quite similar to those set forth in table 2 and table 4 of my aforementioned copending application. A composite substrate employing these components has a coefficient of expansion of about 82.times.10.sup.-7 /.degree.C.
Another glass which may be employed has 40% lead oxide, 20% barium oxide and 40% silicon dioxide and when compounded, as above, provides a composite substrate having a coefficient of expansion of about 46.times.10.sup.-7 /.degree.C.
From the foregoing it is now apparent that a novel composite substrate, as well as a novel method for fabricating a substrate from alternate layers of porcelain tape and wire screen, have been disclosed meeting the objects and advantageous features set out hereinbefore as well as others and that modifications as to the precise configuration, shapes and details may be made by those having ordinary skill in the art without departing from the spirit of the invention or the scope thereof as set out by the claims which follow.