Example I
This example describes the preferred procedure for preparing a beta-hydroxythioether corrosion inhibitor.
The procedure for preparing the corrosion inhibitor is as follows: Chemically-equivalent amounts of EPON.RTM. 828 and beta-mercaptoethanol are dissolved in a 1:1 weight/weight mixture of xylene and methanol. This solution is stirred at ambient temperature to ensure thorough mixing of all components and is then stored at ambient temperature for about 55 hours. Alternatively, the solution is refluxed at about 68.degree. C. for 7 hours to complete the reaction between the mercaptan and epoxide groups. The reaction product possesses a sweet odor rather than a mercaptan odor. The entire reaction mass can be stored in drums until used in the field. The molar ratio of epoxy resin to mercaptoalcohol in the procedure is about 0.5:1 (1 equivalent of epoxide per equivalent of mercaptan).
The course of the reaction used to prepare the corrosion inhibitor can be followed by infrared (lR) spectral analysis. The IR peak due to the presence of the --SH group in the mercaptan reactant becomes less intense and essentially disappears as the thioether is formed. The inventive inhibitor can be prepared by blending chemicals and allowing them to set for 3 to 5 days at ambient conditions or by refluxing the reactants at about 68.degree. C. for seven hours. In either method the reaction product mass possesses essentially none of the unpleasant mercaptan odor. Based on correlation with the infrared spectral data, the formation rate of the corrosion inhibitor is estimated below.
Example Ii
A series of laboratory corrosion inhibition tests was carried out in 1-liter Erlenmeyer flasks equipped with magnetic stirring bars, under laboratory conditions designed to simulate corrosive oil-water environments encountered in field drilling sites. A charge of 50 mL of NBU crude oil and 950 mL of a synthetic brine was used in each run along with the corrosion inhibitor. A slow stream of carbon dioxide was bubbled through the solution during each test to maintain the mixture near saturation with CO.sub.2 at ambient conditions. The rate of corrosion and pitting index were determined using a CORRATOR.RTM. monitoring system available from Rohrback Instruments. A carbon steel probe was suspended in the stirred oil-water mixture maintained at about 49.degree. C. during each run.
A control run (run No. 1 in Table I) using beta-mercaptoethanol was carried out and compared to duplicate inventive runs (runs 2 and 3 in Table I) using the reaction product of beta-mercaptoethanol and EPON.RTM. 828 prepared in a mixture of xylene and methanol. Preparation of the inventive composition was as described in Example 1.
In run No. 1, 0.1 mL of beta-mercaptoethanol was used with 50 mL North Burbank Unit (NBU) crude oil and 950 mL of synthetic NBU brine. In runs 2 and 3, 0.2 mL aliquots of the inventive mercaptoethanol/EPON.RTM. 828 reaction mass in solvent were used with 50 mL NBU crude oil and 950 mL of NBU synthetic brine. In order to test the relative durability of the protective films laid down by the control system and the inventive system, the oil and brine in the test vessels were replaced with fresh oil and brine after about 20 hours, and then the oil-brine test medium was replaced with fresh brine after about 94 hours. The test was terminated after about 116 hours. The results are summarized in Table I.
Referring to the test time interval of zero to 20 hours, it is evident that the control run No. 1 (beta-mercaptoethanol) is comparable in performance (see C.R./P.I. values) to the inventive runs 2 and 3 (reaction product of EPON.RTM. 828 and beta-mercaptoethanol). After the replacement of the oil and brine in all the test vessels at approximately 20 hours, the C.R. and P.I. values for the three runs remained comparable (see time interval of 20 to 94 hours).
Referring to the test interval of 95 to 116 hours after replacing the oil and brine with fresh brine, the C.R. and P.I. values in control run 1 exhibited a significant increase whereas these values in runs 2 and 3 remained relatively low. This replacment of oil and brine with fresh brine alone (at about 94 hours of testing) is a severe test and the lower C.R. and P.I. values for the inventive runs demonstrate the superior film durability of the inventive system.
Example Iii
This example demonstrates the effectiveness of the beta-hydroxythioether corrosion inhibitor system even in the presence of polymeric viscosifiers such as polyacrylamide. The inventive composition was prepared in a 50/50 wt/wt solvent blend of xylene and methanol. A foul-smelling beta-mercaptoethanol and EPON.RTM. 828 were present in a molar ratio of 2:1 (1 equivalent of mercaptan for each equivalent of epoxide) and the mixture was heated at reflux for a period of 24 hours. Aliquots of the pleasant-smelling reaction product mixture were used in the corrosion tests. The laboratory tests were carried out with a CORRATOR.RTM. as described in Example II and the results are summarized in Table II.
Referring to the results in Table II, it is apparent that the inventive composition reduced the corrosion rate to the low value of 0.01 in a very short time. Contacting the coated probe with polyacrylamide resulted in a small increase in corrosion rate (up to 0.9) which was reduced to 0.06 by retreatment with the inventive composition.
At this point (about 24 hours), the coated probe was contacted with another fresh sample of oil and brine and the corrosion rate over a 20 hour span did not exceed 0.56 and was 0.07 after an additional 20 hours of testing.
The final stage of testing was the most severe, as the coated probe was immersed in brine. Over an additonal 20 hours of testing, the maximum corrosion rate increased to 4.9 but then gradually decreased to a final recorded value of 2.8 mpy. These results indicate the superior effectiveness of the instant composition compared to fatty amine corrosion inhibitors, which are known to be readily stripped from metal surfaces on being contacted with aqueous polyacrylamide.
Example Iv
This example describes the preparation of betahydroxythioethers by the thermal condensation of beta-mercaptoethanol (BME) and Epon.RTM. 828 (an epoxy resin). The materials were prepared by refluxing mixtures of xylene, methanol, Epon.RTM. 828 and BME under a nitrogen blanket for approximately 7 hours in conventional laboratory glassware. Four batches of material were prepared at successively higher molar ratios of resin to mercaptoethanol in order to establish the effect of increasing levels of resin on the composition's effectiveness as a corrosion inhibitor. The preparative runs are summarized in Table III.
Example V
This example gives corrosion inhibitor test results for the materials prepared in Example IV. Aliquots of the entire reaction mass were used. The results are summarized in Table IV.
Referring to the results in Table IV, it is evident that the corrosion rates of runs 5, 6, 7 and 8 are comparable even though runs 6, 7, and 8 contained "excess" epoxy resin. These results indicate that the presence of "excess" epoxy resin, i.e., greater than 1:1 equivalent ratio of resin to BME, does not significantly enhance the corrosion inhibiting effectiveness of the formulation.
Example Vi
This example gives additional corrosion inhibitor test results for the materials prepared in Example IV. These results are summarized in Table V.
Referring to the results in Table V, corrosion rate increased as the amount of "chemically combined" beta-mercaptoethanol (beta-hydroxythioether) decreased. The total amount of "chemically-combined" BME and resin was approximately constant (about 76 mg) in runs 9, 10, 11 and 12. This observation indicates that the "chemically-combined" BME species is the likely active inhibitor. Presumably, the deposit on the probe increases as the excess epoxy resin increases successively in runs 9, 10, 11 and 12 which in field applications could lead to "gunk" formation.
Example Vii
This example describes the preparation and testing of a corrosion-inhibiting composition comprising the product resulting from the reaction of n-butyl glycidyl ether and beta-mercaptoethanol in a mixture of xylene and methanol.
A charge of 2.28 g (17.5 mmoles) of n-butyl glycidyl ether, 1.56 g (20 mmoles) of beta-mercaptoethanol and 3.84 g of a 1:1 wt/wt mixture of xylene and methanol was placed in a 25 mL round-bottomed flask fitted with a water-cooled reflux condenser, and the mixture was boiled for about 48 hours under a nitrogen atmosphere. The cooled reaction mixture was essentially free of any mercaptan-like odor. Presumably, the course of the reaction was as follows: ##STR12##
Corrosion tests were carried out on the reaction mass in the same manner as described above. Duplicate samples were tested and the results are summarized in Table VI. The CORRATOR.RTM. test runs involved the use of 0.2 mL aliquots of the reaction mass, 50 mL NBU crude oil and 950 mL of NBU brine.
Referring to the results in Table Vl (duplicate samples in runs and 2), it is evident that the reaction mass resulting from the chemical reaction of beta-mercaptoethanol and n-butyl glycidyl ether is an effective corrosion inhibitor. This example demonstrates that an effective inhibitor can be prepared by reacting essentially equivalent amounts of monomercaptan with the nonpolymeric monoepoxide. Preferably, equivalent amounts of monoepoxide and monomercaptan are desired. However, a slight excess of monoepoxide can be used with no detrimental effects.
Example Viii
This field test example demonstrates the corrosion-inhibiting effectiveness of the reaction mass resulting from the reaction of beta-mercaptoethanol and EPON.RTM. 828 in a mixture of xylene and methanol. The field test was carried out in a polymerflooded area in which the formation water contained significant levels of polyacrylamide. Weight loss of metal coupons was the basis ior determining the corrosion rate in mils per year (mpy). The field test results are summarized in Table VII. Nine wells were tested and the corrosion inhibitor was metered in continuously during the test period. The inventive inhibitor was continuously injected into the wells at the average of about 6 quarts per day.
Referring to the results in Table VII, it is evident that the inventive corrosion inhibitor composition was comparable or superior in performance to the comparison commercial inhibitors. Compare, for example, the magnitude of the corrosion rates under the "Initial Corrosion Rate" heading and the corrosion rates under the heading "Period IV" for the individual wells. In general, four coupons were positioned in each test well and then removed for weighing at time intervals of 37, 72, 96 and 123 days. Entries 3, 4, 5 and 8 in Table VII demonstrate that, of the comparison inhibitors in those wells, were comparable in effectiveness to the inventive composition (comparing corrosion rates, respectively, under the headings "Initial Corrosion Rate" and "Period IV"). Entries 1, 2 and 6 in Table VII demonstrate the dramatic superiority of the inventive composition over the comparison inhibitor (comparing corrosion rates under "Initial Corrosion Rate" and "Period IV").
Example Ix
This example describes laboratory test results using the reaction product of beta-mercaptoethanol/EPON.RTM. 828 g as a corrosion inhibitor in an aqueous medium containing polyacrylamide. Control runs with commercially available corrosion inhibitors designated hereinbelow as "A" and "B" were also carried out in the CORRATOR.RTM. apparatus.
Test solutions initially contained 50 mL NBU crude oil, 950 mL synthetic NBU water and 50 ppm polyacrylamide. Sufficient quantities of inhibitors were added as solutions to give 50 ppm (by volume) levels of "inhibitors" based on volumes of inhibitor solutions added to the test solution. For example, a 0.05 mL aliquot of a commercially available corrosion inhibitor solution added to 1000 mL of test solution gives a "50 ppm level" of said inhibitor solution in the test mixture. Results on duplicate samples are summarized in Table VIII.
Referring to the corrosion rate results in Table VIII, it is seen that the invention inhibitor lowered the corrosion rate more rapidly and to lower ultimate values than did the commercial inhibitors "A" and "B". It is also noteworthy that the corrosion rate for the invention systems continued to decrease even after the addition of more polyacrylamide at the 25.5 hour and 26.5 hour time intervals in the test procedure.
Example X
This example demonstrates the biocidal activity of the reaction product of beta-mercaptoethanol and EPON.RTM. prepared in a xylene/methanol mixture. A 200 ppm concentration of the adduct solution in methanol was effective against sulfate-reducing bacteria. The methanol solution was prepared by adding a sufficient amount of a stock solution of product in 1:1 xylene/methanol to methanol to give a 200 ppm by volume) level of corrosion inhibitor solution in methanol.
Control tests with methanol and the reaction product of an amine and an epoxy resin proved ineffective toward sulfate-reducing bacteria. The amine/epoxy resin corrosion inhibitor was prepared by contacting aliquot quantities of EPON.RTM. 828 and DUOMEEN.RTM. T in a xylene/methanol (1:1 wt/wt) mixture and then contacting the mixture with carbon dioxide. The methanol test solution of the amine/epoxy corrosion inhibitor system was prepared by adding a sufficient amount of a stock solution of inhibitor in 1:1 xylene/methanol to methanol to give a 200 ppm (by volume) level of corrosion inhibitor solution in methanol. Results are summarized in Table IX.
Referring to the results in Table IX, it is evident that the sulfur-containing corrosion inhibitor (first entry) exhibited biocidal activity toward sulfate-reducing bacteria. The second and third entries of Table IX indicate the ineffectiveness, respectively, of the nitrogen-containing corrosion inhibitor and methanol toward sulfate-reducing bacteria. In view of these results, it can be inferred that the protective film of the beta-hydroxythioether corrosion inhibition system would not be subject to degeneration by SRB attack and therefore would provide corrosion inhibition over a longer period of time than an inhibitor film which was not biocidal toward sulfate-reducing bacteria.
Example Xi
This example describes corrosion inhibitor laboratory test results using a beta-hydroxythioether and a quaternized polyethoxylated amine.
The beta-hydroxythioether used in this example resulted from the stoichiometric reaction of Epon.RTM. 828 and beta-mercaptoethanol in a mixture of xylene and methanol. The reaction was carried out so that the beta-hydroxythioether inhibitor solution was the total reaction mass resulting from the reaction of equivalent quantities of Epon.RTM. 828 and beta-mercaptoethanol in a 1:1 wt/wt mixture of xylene and methanol wherein the total weight of the charged reactants was equal to one-third of the total reaction mass.
The quaternary salt adjuvant was a commercially available polyethoxylated quaternary ammonium salt sold under the trademark Ethoquad.RTM. C/25. This material is 95% active methylpolyoxyethylene(15)cocoammonium chloride and is commercially available as a clear liquid.
Laboratory corrosion inhibitor tests were carried out in 1-liter Erlenmeyer flasks. The corrosion inhibitor to be tested was added to 50 mL of NBU crude oil and this mixture was transferred to a 1-liter Erlenmeyer flask containing 950 mL of NBU brine. A slow stream of CO.sub.2 was passed through the oil-water system to maintain a slight positive pressure of carbon dioxide. For the runs summarized in Table X the oil-water mixture was stirred continuously with a magnetic bar. The rate of corrosion in terms of mils per year (mpy) was determined using a Corrator.RTM. monitoring system available from Rohrback Instruments. A carbon steel probe was suspended in the oil-water mixture maintained at approximately 49.degree. C. during each run.
BHTE represents beta-hydroxythioether produced by the reaction of equivalent quantities of Epon.RTM. 828 and beta-mercaptoethanol in a 1:1 wt/wt mixture of xylene and methanol wherein the combined weights of Epon.RTM. 828 and beta-mercaptoethanol amounted to one-third of the total reaction mass. One part by weight of this reaction mass was combined with one part of methanol to form the BHTE solution used in the corrosion tests.
C/25 represents Ethoquad.RTM. C/25, which is a 95% active commercial material of methylpolyoxyethylene(15)cocoammonium chloride (a quaternary salt). Appropriate amounts of (C/25)/methanol stock solutions were used in the corrosion tests.
BHTE/(C/25) represents a mixture of the beta-hydroxythioether (see above) and the 1/4 (C/25)/methanol stock solution of (b). One part of the reaction mass containing the beta-hydroxythioether in (a) was combined with one part of the 1/4 (C/25)/methanol stock solution of (b) for use in the corrosion tests.
Results of the corrosion tests are summarized in Table X.
The levels of inhibitor in the corrosion tests are deiined as follows, based on a 1000 mL volume of test mixture containing about 50 mL NBU crude oil and about 950 mL of NBU brine, e.g.,
Referring to the results in Table X, the BHTE/(C-25) inventive composition at 25 ppm (run 3) gave lower corrosion rates in a shorter time (see 4-hour results) than did either the BHTE system (run 1) or the C-25 system (run 2). At the higher level of 50 ppm for the BHTE/(C-25) system (see duplicate runs 4 and 4a), the improvement is also apparent. These runs demonstrate that the effectiveness of the beta-hydroxythioether system for corrosion inhibition is enhanced by the inclusion of the quaternary salt adjuvant.
Example Xii
This example describes corrosion inhibitor laboratory test results using the beta-hydroxythioether described in Example XI mixed with polyoxyethylene(15)cocoamine (an amine) and trimethylcocoammonium chloride (50% active) (quaternary salt). A stock solution for corrosion testing was prepared by mixing the following three components:
(a) 20 mL BHTE (beta-hydroxythioether solution resulting from the reaction of Epon.RTM. 828 and beta-mercaptoethanol in a 1:1 wt/wt mixture of xylene and methanol).
(b) 10 mL Ethomeen.RTM. C/25 (a commercially available polyoxyethylene(15)cocoamine).
(c) 10 mL Arquad.RTM. C-50 (a 50% active commercially available trimethylcocoammonium chloride quaternary salt in aqueous isopropanol).
Laboratory corrosion inhibitor tests were carried out with the three-component stock solution to demonstrate its effectiveness in the presence or absence of polyacrylamide. The results of these tests are summarized in Table XI.
Referring to duplicate runs 5 and 6 in Table XI, the beta-hydroxythioether-polyethoxylated amine-quaternized amine lowered the corrosion rate almost immediately to an average value of <0.5 mpy. Duplicate runs 1, 2 and 3, 4 at 50 and 200 ppm levels, respectively, required somewhat longer times (on the order of 5-6 hours) to lower the corrosion rate to values of less than 1.5 mpy in systems containing about 1000 ppm polyacrylamide. All of the systems in Table XI exhibited corrosion rates of less than 1 mpy even after 28 hours of testing.
It is noteworthy that the corrosion inhibitor system was effective in the presence of polyacrylamide, since polyacrylamides on contacting nitrogen-based corrosion-resistant films often remove the films, necessitating frequent retreatment.
Example Xiii
This example describes corrosion inhibitor laboratory test using different levels of a 1:1 wt/wt solution of BHTE and Ethoquad C/25 wherein (a) BHTE and (b) Ethoquad.RTM. C/25 represent, respectively, (a) beta-hydroxythioether solution produced by the reaction of equivalent quantities of Epon.RTM. 828 and beta-mercaptoethanol in a 1:1 wt/wt mixture of xylene and methanol wherein the combined weights of Epon.RTM. 828 and beta-mercaptoethanol amounted to one-third o: thc total reaction mass and (b) a 95% active commercially available methylpolyoxyethylene(15)cocoammonium chloride (a quaternized polyoxyethylene(15)cocoamine). The 1:1 wt/wt test solution of BHTE and Ethoquad.RTM. C/25 is designated BHTE/EQ.
The corrosion test levels of inhibitor solution at 10 ppm, 25 ppm and 50 ppm were formulated by adding, respectively, 0.01 mL, 0.025 mL and 0.05 mL of the 1:1 wt/wt BHTE/Ethoquad C/25 stock solution to a 1000 mL volume of test mixture containing about 50 mL NBU crude oil and about 950 mL of NBU brine. Results are summarized in Table XII.
Referring to the results in Table XII, the beta-hydroxythioether/quaternary salt system (BHTE/EQ) lowered the corrosion rate almost immediately to an average value of less than 0.10 mpy. The corrosion rates were maintained at very low levels even after 14 hours of testing. The system was very effective even at 10 ppm (runs 1 and 2).
Example Xiv
This example demonstrates that a quaternary salt adjuvant such as a quaternary ammonium salt of a long chain alkenyl succinate enhances the corrosion inhibiting effectiveness of a beta-hydroxythioether.
The corrosion inhibitor tests were carried out in essentially the same manner as described above. The beta-hydroxythioether was produced by the reaction of equivalent quantities of Epon.RTM. 828 and beta-mercaptoethanol in a 1:1 wt/wt mixture of xylene and methanol in which the combined weights of Epon.RTM. 828 and beta-mercaptoethanol amounted to one-third of the total reaction mass. Samples of the reaction mass solution were used in the tests.
The tests employed a mixture of a commercially available corrosion inhibitor (ASQ), which is a quaternary salt of an alkenyl succinate, with the beta-hydroxythioether (BHTE) solution. The mixture contained 90 volume percent of the BHTE solution and 10 volume percent of the ASQ solution.
The corrosion test level for the BHTE solution was 200 ppm based on the volume percent of added BHTE solution to the total test mixture of 1000 mL, i.e., 50 mL NBU crude oil and about 950 mL of NBU brine. A 0.2 mL aliquot was used in order to obtain the 200 ppm concentration level. Similarly, in testing the BHTE/ASQ mixture, a 0.2 mL aliquot was used in order to obtain a 180 ppm level of the BHTE solution and 20 ppm level of the commercial solution of ASQ (a quaternary salt of an alkenyl succinate). The results of the corrosion tests are summarized in Table XIII.
Referring to the results in runs 1 and 2, the BHTE/ASQ mixture was more effective than the BHTE solution alone particularly after the addition of 1000 ppm of polyacrylamide stock solution to the test system. The addition of the polyacrylamide caused the corrosion rate in the BHTE test (run 1) to increase from about 0.01 mpy to about 0.7 to 0.9 mpy whereas in the BHTE/ASQ system (run 2) the corrosion rate remained at about 0.01 mpy even after addition of polyacrylamide.
Run 3 in Table XIII demonstrates the corrosion inhibiting effectiveness of the commercial quaternary salt both before and after the addition of polyacrylamide. lt is known that polyacrylamides on contacting nitrogen-based corrosion-resistant films can remove the films, necessitating frequent retreatment.