Background of the Invention
1. Field of the Invention
This invention relates to integrated circuit production, and more particularly to a method for enhancing the electronic properties of silicon dioxide insulating layers in metal oxide semiconductor devices, decreasing hole trapping and thereby increasing radiation hardness, by a rapid thermal annealing of the integrated circuit wafer at a stage during production when the silicon dioxide insulating layer is exposed.
2. Description of the Prior Art
The prior art techniques for enhancing the electronic properties of silicon dioxide insulating layers in metal oxide semiconductor (MOS) devices includes the use of long anneals at 1000 C.
The prior art techniques do not teach nor suggest the rapid thermal annealing of silicon dioxide insulating layers in MOS device wafers, but rather require very long anneals, which do not provide the desired enhancement of electronic properties.
Various thermal treatments of semiconductor materials, as contrasted to thermal treatments of silicon dioxide insulating layers, are known in the prior art. Such treatments have application in healing ion implantation damage, in activating implanted dopants, and in other mechanisms affecting semiconductor properties; there is however no unified theory of thermal treatments which might predict success of a short anneal of silicon dioxide insulating layers.
Summary of the Invention
Therefore, it is an object of the present invention to enhance electronic properties of silicon dioxide, to reduce hole trapping and thereby increase radiation hardness and improve the dielectric breakdown properties.
A feature of the invention is rapid heating of a semiconductor chip or wafer by controlled application of radiation from a high intensity halogen lamp, so as to carry out an annealing process without disruption of other processes or long waiting periods.
The advantage of the invention is its high quality and convenience; its production of the desired enhancements, increased radiation hardness and reduced hole trapping, are achieved without the extra effort and additional chance of contamination or unwanted diffusion inherent in longer anneals.
The foregoing and other objects, features and advantages of the invention will be apparent from the more particular description of the preferred embodiments of the invention, as illustrated in the accompanying drawing.
Brief Description of the Drawings
FIG. 1 is a schematic diagram of appropriate apparatus.
FIG. 2 is a graph showing hole trapping.
Description of a Preferred Embodiment of the Invention
The invention is a process for providing reduced hole trapping characteristics to a silicon dioxide insulator film on a MOS integrated circuit wafer. FIG. 1 shows typical apparatus. The silicon semiconductor wafer 1 has silicon dioxide insulator 2 on its surface, which surface will subsequently have conductors deposited upon it. The wafer is supported on a quartz plate 3 and inserted into a quartz enclosure 4. The desired gas is flown into this enclosure at inlet port 5; the gas escapes at exit port 6. An array of lamps 7, which are typically tungsten halogen lamps, are turned on to heat wafer 1 rapidly to the desired annealing temperature for a short time.
The anneal of a silicon dioxide film of thickness on the order of 100-1000 Angstroms is carried out in an atmosphere of oxygen at atmospheric pressure. The preferred temperature and duration are 1000 C for 100 seconds; the range 10-300 seconds is effective, with a peak around 100 seconds.
FIG. 2 shows the reduction in hole trapping achieved by the rapid thermal annealing; it is a graph of flatband voltage shifts as a function of hole injection time in MOS capacitor structures. The flatband voltage shifts are proportional to the amount of hole trapping in the silicon dioxide. The control curve shows high trapping in oxides before annealing. Other curves, labeled with annealing time for rapid thermal annealing (RTA) show improvement in the form of reduced hole trapping. In particular, the curve for 100 seconds shows drastically reduced hole trapping, approaching the 0 trapping level.
Improved RTA annealing characteristics are found when the RTA is subsequent to a nitrogen pretreatment, such as a long post oxidation anneal in nitrogen, which provides nitrogen atoms at the silicon-silicon dioxide interface. Such nitrogen pretreatment may typically be a post-oxidation anneal (POA) of seventeen hours in nitrogen at 1000 C.