US 4,543,305 AGrant
Method of Pretreating Carbon Black Powder to Improve Cathode Performance and Lithium Sulfuryl Chloride Cell Including the Pretreated Carbon Black Powder
Issue Date:1985-09-24
•6 Claims
•1 Drawing Sheets
Abstract
Carbon black powder is pretreated with acetone or methanol prior to cathode abrication to improve the cathode operating voltage and increase the cathode life of lithium sulfuryl chloride electrochemical cells.
Metadata
Assignee
- The United States of America as represented by the Secretary of the Army
Inventors
- Michael Binder
- Charles W. Walker, Jr.
- Eric R. Petersen
- William L. Wade, Jr.
- Sol Gilman
Application Information
Application Number:US 7158084
Filing Date:1985-03-25
Priority Date:1983-10-24
Art Unit:114
Classifications
IPC:
H01M 496H01M 614
Field of Search:
429423101;196;218;209460
Patent Drawings (1 sheets)
Description
Description of the Drawing and the Preferred Embodiment
FIG. 1 shows constant current discharge curves for carbon cathodes in Li/1.5 M LiAlCl.sub.4 --SO.sub.2 Cl.sub.2 cells fabricated from Shawinigan acetylene black with and without acetone pretreatment.
FIG. 2 shows constant current discharge curves for carbon cathodes in Li/1.5 M LiAlCl.sub.4 --SO.sub.2 Cl.sub.2 cells fabricated from a high surface area carbon, CSX-179B carbon black with and without acetone pretreatment.
Referring to FIG. 1, best performance in terms of high operating load voltages and cathode capacity appears to be obtained for cathode constructed with acetone pretreated carbon blacks.
In fact, cathodes fabricated with the pretreated carbon black have capacities comparable to cathodes fabricated with high surface area carbon.
This result is entirely unexpected. It would not be expected that a relatively mild room temperature treatment with a fairly volatile substance that is subsequently removed could effect as dramatic a change in cathode performance. In general, vigorous reduction or oxidation at temperatures in excess of 750.degree. C. is required in order to oxidize or reduce surface chemical groups.
In order to determine whether this observed improvement could be peculiar to Shawinigan acetylene black, similar experiments were performed on a high surface area carbon CSX-179B with a surface area of 1500 m.sup.2 /g and the results are shown in FIG. 2. It is clear that substantial improvements are achieved by simple treatment. Again the improvements are unexpected since the two carbons tested differ substantially in surface area, pH, ash content and percent impurity.
It is thus evident that pretreatment of both Shawinigan acetylene black and CSX-179B with acetone subsequently yielded cathodes that showed marked improvements in both operating voltages and capacities over untreated baseline cathodes.
This pretreatment method of the invention is considered to be applicable to any battery or fuel cell system where carbon black is used as an electrode material.
We wish it to be understood that we do not desire to be limited to the exact details as described for obvious modifications will occur to a person skilled in the art.
Claims
What is claimed is:
1. A lithium sulfuryl chloride electrochemical cell including polytetrafluoroethylene bonded carbon cathodes and having an improved cathode operating voltage and an increased cathode life, said improvements being obtained by pretreating the carbon black powder with acetone prior to cathode fabrication.
2. A lithium sulfuryl chloride electrochemical cell according to claim 1 wherein the carbon black powder is a low surface area carbon black powder.
3. A lithium sulfuryl chloride electrochemical cell according to claim 2 wherein the carbon black powder is a high surface area carbon black powder.
4. A lithium sulfuryl chloride electrochemical cell including tetrafluoroethylene bonded carbon cathodes, and having an improved cathode operating voltage and an increased cathode life, said improvements being obtained by pretreating the carbon black powder with acetone prior to cathode fabrication, filtering the carbon black-acetone mixture through a Buchner funnel fitted with a filter paper, rinsing with an excess amount of water and drying overnight in a vacuum oven at about 100.degree. C.
5. A lithium sulfuryl chloride electrochemical cell according to claim 4 wherein the carbon black powder is a low surface area carbon black powder.
6. A lithium sulfuryl chloride electrochemical cell according to claim 4 wherein the carbon black powder is a high surface area carbon black powder.