The present invention will be illustrated with reference to the following examples and comparative examples, which are however given for the purpose of illustration and are not to be interpreted as limiting the present invention.
EXAMPLE 1
To a polymerization vessel having an anchorform mixing blade with a small clearance between the blade and its internal wall surface, were added 910.8 g (6.6 moles) of p-hydroxybenzoic acid, 547.8 g (3.3 moles) of terephthalic acid, 606.4 g (3.26 moles) of 4,4'-dihydroxydiphenyl, 5.0 g (0.04 mole) of 1,3,5-trihydroxybenzene and 1,485 g (14.56 moles) of acetic anhydride. The resulting mixture, with stirring in a nitrogen atmosphere, was heated to 150.degree. C. and refluxed for 3 hours at this temperature. Thereafter, while raising the temperature, acetic acid resulting from reaction was distilled off, and the temperature was finally raised to 310.degree. C. under high shear. The polymerization was continued for another two hours with powerful stirring, and the reaction mixture was then cooled to 200.degree. C. to obtain 1,736 g (94.6%) of a polymer.
The polymer was pulverized so as to pass through a 0.5 mm-mesh screen and transferred to aluminum rotary oven. Thereafter, while rotating the whole system in a nitrogen stream and thoroughly stirring the powder, the powder was heated to 330.degree. C. over 6 hours, treated at 330.degree. C. for 3 hours, cooled and taken out at 200.degree. C.
This polymer was granulated on a single-screw extruder VS-30-28 (screw diameter, 30 mm; L/D, 28; produced by Tanabe Plastic Machinery Co.) under a condition that the cylinder temperature be 350.degree. C. and the number of rotations of the screw be 50 rpm, and then injection-molded on Neomat N 47/28 (injection molding machine produced by Sumitomo Shipbuilding & Machinery Co.). Various test pieces were molded, and the values of the respective physical properties were measured.
The result is shown in Table 1. The surface roughness of the molded product by orientation is inhibited, and the appearance is also smooth. Processability on molding is also good, this being apparent from the large strength of the welded part.
Hereupon, as a mold for the evaluation of welded parts, there was used a window frame-form mold having its gate at the center so as to produce welded parts, and the molded product produced by it was 3 mm in thickness, 12.5 mm in width and 64 mm in the outside length of each side.
The results of Examples 2, 3 and 4 and Comparative Example 1 are also shown in Table 1.
EXAMPLES 2, 3 and 4
The results of the systems wherein the amounts of 1,3,5-trihydroxybenzene are 0.5 mole %, 3 mole % and 6 mole %, respectively, based on the total amount of 1,3,5-trihydroxybenzene and 4,4'-dihydroxydiphenyl, are shown in Table 1.
COMPARATIVE EXAMPLE 1
The result of the system containing no 1,3,5-trihydroxybenzene is shown in Table 1. The orientation of the molded product is large, the welding of parts to be welded being difficult, so that the strength of the welded part is also small.
COMPARATIVE EXAMPLE 2
Using the same apparatus as used in Example 1, 910.8 g (6.6 moles) of p-hydroxybenzoic acid, 531.2 g (3.2 moles) of terephthalic acid, 613.8 g (3.3 moles) of 4,4'-dihydroxydiphenyl, 19.2 g (0.1 mole) of trimellitic anhydride and 1,485 g (14.56 moles) of acetic anhydride were added to the apparatus and treated in the same manner as in Example 1 to obtain 1,741 g (97.9 %) of a polymer. Thereafter, the polymer was heat-treated, granulated and molded in the same manner. With a molding temperature of 390.degree. C., the tensile strength was 1,210 kg/cm.sup.2 ; tensile modulus, 3.9.times.10.sup.4 kg/cm.sup.2 ; and bending strength of the welded part was 120 kg/cm.sup.2. It can be seen from this result that the bending strength shows a somewhat improved value as compared with Comparative Example 1, but that the effect is small as compared with Examples 1, 2, 3 and 4.
EXAMPLE 5
Using the following feed condition, a polymer was synthesized in the same manner as in Example 1: p-Hydroxybenzoic acid, 910.8 g (6.6 moles); terephthalic acid, 547.8 g (3.3 moles); 4,4'-dihydroxydiphenyl, 606.4 g (3.26 moles); 3,5-dihydroxybenzoic acid, 12.32 g (0.08 mole; 1 mole %, as phenol, based on 4,4'-dihydroxydiphenyl); and acetic anhydride, 1,485 g (14.56 moles).
On producing a molded product by the same treatment and molding, it was found that the surface roughness by orientation was inhibited and the appearance was also good as compared with a case wherein 3,5-dihydroxybenzoic acid was not added, and that the molded product obtained at 390.degree. C. had well-balanced physical properties as shown by a tensile strength of 1,030 kg/cm.sup.2, tensile modulus of 3.7.times.10.sup.4 kg/cm.sup.2 and a bending strength of welded part of 380 kg/cm.sup.2.
COMPARATIVE EXAMPLE 3
In order to examine the effect of pyrogallol triacetate as used in EXAMPLES of U.S. Pat. No. 4,417,043, the following experiment was carried out:
The polymerization was carried out according to the method of Example 1 except that 5.0 g (0.04 mole) of pyrogallol (1,2,3-trihydroxybenzene) was used in place of the 1,3,5-trihydroxybenzene to evaluate the obtained polymer by the molded product as in Example 1. In this case, the pyrogallol was allowed to react with the acetic anhydride to form pyrogallol triacetate as a transient intermediate. The injection molding was carried out at 360.degree. C., the appearance of molded product showed silver streaks caused by molecular orientation, the heat stability was poor compared with that of no incorporation of the pyrogallol, and outgassing was observed during the molding.
Tensile strength, tensile modulus and bending strength of welded part of the molded product were 1350 kg/cm.sup.2, 4.1.times.10.sup.4 kg/cm.sup.2 and 58 kg/cm.sup.2, respectively, and accordingly, no effect of the pyrogallol triacetate was observed.