Cross-Reference to Related Applications
John F. Bates et al., copending application Ser. No. 414,167 filed on Sept. 2, 1982, entitled "Austenitic Alloy and Reactor Components Made Thereof" pertains to austenitic stainless steels containing increased levels of phosphorus to provide enhanced inreactor swelling resistance. The specification of this application is hereby incorporated by reference.
The present invention relates to austenitic stainless steels for use in high temperature applications. More particularly, the present invention especially relates to austenitic stainless steel alloys for use in nuclear reactor applications.
One of the prime objectives in the efforts to develop a commercially viable liquid metal fast breeder reactor (LMFBR) has been to develop an alloy, or alloys, which are swelling resistant and have the required inreactor mechanical properties for use as fuel cladding and/or use as ducts. The fuel cladding will see service in contact with flowing liquid sodium and have a surface temperature of about 400.degree. C. (.about.750.degree. F.) to 650.degree. C. (.about.1200.degree. F.). A duct surrounds each bundle of fuel pins and sees service at about 380.degree. C. (.about.715.degree. F.) to 550.degree. C. (.about.1020.degree. F.). These components will be exposed at the aforementioned elevated temperatures to fast neutron fluxes on the order of 10.sup.15 n/cm.sup.2 .multidot.S (E>0.1 MeV), and should be capable of performing adequately to fluences on the order of 2 to 3.times.10.sup.23 n/cm.sup.2 (E>0.1 MeV).
Initially, one of the prime candidate alloys for commercial LMFBR, fuel cladding and ducts was 20% cold worked AISI 316 steel, a solid solution strengthened austenitic stainless steel (see Bennett and Horton, "Material Requirements for Liquid Metal Fast Breeder Reactor," Metallurgical Transactions A, Vol. 9A, February 1978, pp. 143-149). Typical chemistry and material fabrication steps for nuclear grade 316 fuel cladding are described in U.S. Pat. No. 4,421,572 filed on Mar. 18, 1982. The specification of U.S. Pat. No. 4,421,572 is hereby incorporated by reference.
Current commercial composition specifications for nuclear grade 316 stainless steel contain only a maximum value for impurities such as phosphorus, sulphur, boron, aluminum, niobium, vanadium, tantalum, copper and cobalt. Typical commercial melting procedure for this alloy involves double-vacuum melting of electrolytic-grade starting materials. This practice results in low levels of the aforementioned impurities, which depending on the particular impurity, may be 10 to 100 times less than the maximum value allowed by the specification.
However, the 316 alloy undergoes a high degree of void swelling during extended exposure to fast neutron fluxes at the LMFBR operating temperatures. Extensive development efforts aimed at reducing swelling have been undertaken, and are exemplified by U.S. Pat. No. 4,158,606 and U.S. Pat. No. 4,407,673 filed on Jan. 9, 1980.
While the aforementioned efforts have led to improvements in swelling resistance, the stress rupture behavior of these alloys in fuel pin cladding applications remains as one of the major limitations on fuel pin life and improvements in this area are needed for long-life LMFBR cores.
Applicants have now discovered that in the solid solution strengthened austenitic stainless steels that stress rupture strength increases as the sum of the phosphorus, sulphur and boron contents of the alloy increase. Based on this discovery, applicants have developed alloy compositions having enhanced stress rupture properties and good swelling resistance, making them suitable for use as fuel pin cladding. These alloy compositions are summarized in Table I and utilize phosphorus, boron and sulphur, in conjunction with controlled quantities of selected impurities and a controlled ratio of wt.% titanium to the sum of the wt.% carbon and nitrogen, to provide the desired stress rupture properties.
In accordance with the present invention, it is preferred that within the broad range shown in Table I that the sulphur content be limited to 0.005 to 0.010 wt.%, the phosphorus content be limited to 0.025 to 0.06 wt.%, and the boron content be limited to 0.003 to 0.006 wt.%.
It is also preferred that the Ti/C+N for both the broad and preferred compositions shown in Table I be between 4.5 and 5.5.
While the alloys according to the present invention may be put to good use in any high temperature applications requiring good stress rupture properties in the temperature range of about 500.degree. to 800.degree. C., the present alloys are particularly well suited for use in elevated temperature, high fluence, fast neutron irradiation environments such as those encountered by fuel element cladding in an LMFBR core. In this application, the alloy requires a cold worked microstructure which may be produced by the final cold working step in tube fabrication. A 10 to 40%, and more preferably, a 15 to 25% final reduction in area is desired in the final cold working step.
These and other aspects of the present invention will become more apparent upon a reading of the following detailed specification in conjunction with the figures listed immediately below.
Brief Description of the Drawings
FIG. 1 shows a graph of the stress required to produce rupture in 1000 hours at 650.degree. C. as a function of the sum of the phosphorus, boron and sulphur contents in weight percent;
FIG. 2 shows the effect of varying boron contents on stress rupture life at 700.degree. C. for a stress of 36.6 ksi for three different phosphorus contents;
FIG. 3 shows the effect of varying phosphorus contents on stress rupture life at 700.degree. C. for a stress of 36.6 ksi for three different boron contents; and
FIG. 4 shows stress rupture life at 700.degree. C. under an applied stress of 36.6 ksi as function the (wt.% P).times.(wt.% B).
Detailed Description of the Invention
As demonstrated in FIG. 1, applicants have discovered that stress rupture strength in austenitic stainless steels is a function of the sum of the phosphorus, sulfur and boron contents of the alloy. More particularly, curve 1 shows that the stress required to produce rupture in these alloys in 1000 hours at 650.degree. C. increases substantially linearly with increasing phosphorus, sulphur and boron content.
Based on the relationship between rupture strength and the aforementioned elements disclosed by FIG. 1, it is required that the alloys of the present invention have at least 0.03 wt.%, and preferably at least 0.035 wt.%, total, of boron, phosphorus and sulphur. It is further believed that small, but finite amounts of the impurities niobium, vanadium, tantalum, aluminum, copper, and cobalt, should also be present to provide the desired stress rupture properties. To this end, applicants have set minimum values for each of these elements as shown by Table I.
In addition, in the alloys of the present invention, it is required that the ratio (on a weight percentage basis) of titanium to the sum of carbon and nitrogen be between 4 and 6 and most preferably about 5. It is believed that in the present alloys, the aforementioned Ti/(C+N) ratio range is conducive to placing a large fraction of the carbon and nitrogen atoms in the alloy into fine, Ti(C,N) particles dispersed through the cold worked austenitic matrix. In alloys having the specified Ti/(C+N) ratios, these fine Ti(C,N) particles are expected to be more resistant to coarsening during elevated temperature use and thereby maintain the inhibiting effect these particles have on dislocation motion for longer periods of elevated temperature use at a specific temperature.
In producing the alloys according to the present invention, the electrolytically pure starting materials of the prior art may be partially or entirely replaced by scrap which has been selected to provide a melt chemistry, meeting the requirements of Table I. Any of the melting techniques known in the art may be used in the production of the present alloys so long as they are capable of providing a product meeting the Table I chemistry requirements. Double-vacuum melting is specifically contemplated.
Standard hot working, cold working and annealing techniques used in the prior art may be utilized to fabricate final size components from ingots of the present alloys. Fuel element cladding may be fabricated from hot worked billets by cold working reductions having anneals between each reduction as is described in copending application Ser. No. 414,167 and U.S. Pat. No. 4,421,572. The finished cladding should have a cold worked microstructure produced by a final cold working reduction of about 10 to 40% in cross-sectional area, with reductions of 15 to 25% being preferred.
The invention will be further clarified by a consideration of the following examples, which are intended to be purely exemplary of the invention.
Nine heats having the compositions shown in Table II, with varying boron and phosphorus contents, were melted and fabricated down to round bar stock having a diameter of about 0.53 to 0.532 inches. Prior to the final cold working reduction, the alloys were annealed at about 1066.degree. C. for about 15 minutes and then air-cooled. The final cold working reduction was about 23%.
Stress rupture testing of the final cold worked bars, highlighted an unexpected and surprising interaction between boron and phosphorus contents shown in FIGS. 2 through 4. These Figures indicate that stress rupture lifetime is dependent on a strong interaction between the boron and phosphorus contents in the alloys of the present invention.
FIG. 2 shows lifetime to rupture, at 700.degree. C. and a stress of 36.6 ksi, as a function of boron content for three different levels of phosphorus content. Curve 30 shows that increasing boron content in alloys containing >0.005 wt.% phosphorus while initially producing a small increase in rupture lifetime, does not produce an increase in rupture lifetime above boron contents of 0.0028 wt.%. Curve 20, for alloys containing nominally 0.03 wt.% phosphorus, indicates that increasing the boron content of these alloys results in a substantially linear increase in the rupture life time. Curve 10 for alloys containing nominally 0.085 wt.% phosphorus, indicates that increasing the boron content from 0.0008 wt.% to 0.0029 wt.% results in an approximate tripling of the stress rupture life time. Increasing the boron content from 0.0029 to 0.0064 wt.% results in a further increase in rupture lifetime which is, however, not as large as the increase in going from 0.0008 to 0.0029 wt.%.
FIG. 3, utilizing the same data used to plot the FIG. 2 curves, shows the stress rupture lifetime as a function of phosphorus content for three different levels of boron content. Curve 60, for alloys containing nominally 0.0008 wt.% boron, shows that increasing phosphorus from less than 0.005 wt.% to about 0.03 wt.% produces a small increase in rupture lifetime, but that further increases in phosphorus content do not produce further increases in rupture lifetime. Curve 50, for alloys containing about 0.003 wt.% boron, shows that increasing phosphorus produces an almost linearly increasing stress rupture lifetime from just above 100 hours for less than 0.005 wt.% phosphorus to over 500 hours for about 0.085 wt.% phosphorus. Curve 40, for alloys containing about 0.006 wt.% boron, shows that up to about 0.03 wt.% phosphorus, rupture lifetime increases at a faster rate than in the 0.003 wt.% boron alloys 50, but beyond about 0.030 wt.% phosphorus, the rate of increase in rupture lifetime with phosphorus content is substantially the same as that shown by curve 50 for the same phosphorus content interval.
In FIG. 4, the base ten logarithm of rupture lifetime is plotted as a function of the base ten logarithm of the product of the wt.% phosphorus times the wt.% boron. Curve 100, based on the data used to generate FIGS. 2 and 3, shows that rupture lifetime is a function of the product of the phosphorus and boron content where:
R.sub.L .varies.(wt.% P.times.wt.% B).sup.n
R.sub.L =rupture lifetime
n=slope of curve 100, for T=700.degree. C. and
.sigma.=36.6 ksi
Based on the data shown in FIGS. 2 through 4, it is apparent that: (1) at boron contents of about 0.001 wt.% or less, increasing the phosphorus content from <0.005 to about 0.085 wt.% will not produce any significant change in rupture lifetime; and (2) at phosphorus contents less than 0.02 wt.%, that increasing the boron content will not produce any significant change in rupture lifetime. The present inventors therefore believe that in the present alloys it is critical that there be at least 0.002 wt.% boron and 0.02 wt.% phosphorus present. The maximum boron and phosphorus contents should be maintained below about 0.008 wt.% and about 0.08 wt.%, respectively, to assure the fabricability and weldability of the alloys. To achieve an optimum combination of rupture, fabrication and welding properties, boron should be present at levels of 0.003 wt.% to 0.006 wt.%, and phosphorus should be present between 0.025 wt.% and 0.06 wt.%. Maximum stress rupture lifetime can be obtained by simultaneously maximizing the boron and phosphorus contents within the above ranges. Approximately equivalent stress rupture lifetimes can be maintained between different alloys having varying boron and phosphorus contents within the aforementioned ranges by setting the product of the phosphorus and boron contents of the desired alloy equal to the product of the phosphorus and boron contents of the other alloy.
Other embodiments of the invention will become more apparent to those skilled in the art from consideration of the specification or practice of the invention disclosed herein. It is intended that the specification and examples be considered as exemplary only, with the true scope and spirit of the invention being indicated by the following claims.