Brief Description of the Drawings
The above-mentioned and other features and objects of the present invention, and the manner of attaining them, will become more apparent and the invention itself will be better understood by reference to the following description of an embodiment of the invention taken in conjunction with the accompanying drawings, wherein:
FIG. 1 is a broken-away view of an elongate self-supporting constructional element produced by the method of the present invention;
FIG. 2 is a broken-away view of a core utilized in the method;
FIG. 3 is a broken-away view of a second elongate self-supporting constructional element produced by the method; and
FIG. 4 is a transverse cross-section of the core having an intermediate layer and the deposited self-standing constructional element thereon.
Detailed Description
Referring to the Figures, core 14 made of a suitable material is provided for spraying on its outer surface 26 an intermediate layer 28 made of metallic or non-metallic material. After application of layer 28, self-supporting constructional element 32 is applied to intermediate layer 28. Both layer 28 and element 32 are preferably applied by plasma spraying. As illustrated in FIG. 3, the method of the present invention also contemplates other constructional elements such as crucible 38.
In performing the method of the present invention, core 14 has intermediate layer 28 deposited thereon by plasma spraying. Intermediate layer 28 may be a non-metallic or metallic material, such as aluminum, zirconium, or potassium chloride. Moreover, core 14 can be preheated either before or after deposition of intermediate layer 28, and is preferably preheated to a temperature between about 200.degree. C. to about 650.degree. C. Preheating core 14 permits the method of the present invention to take advantage of the effects of thermal expansion in the subsequent removal of element 32.
Thereafter, self-supporting constructional element 32, or crucible 38, is deposited on intermediate layer 28 by plasma spraying. Constructional element 32, or crucible 38 is made of a ceramic oxide, such as zirconium silicate or aluminium oxide.
After constructional element 32, or crucible 38, has been applied on intermediate layer 28 to a desired thickness, core 14 is cooled and intermediate layer 28 is removed therefrom. Layer 28 can be removed by application of a solvent, such as acid, water, or by fusion. The method of removing intermediate layer 28 will depend upon the material of which it is made.
When core 14 has been cooled and intermediate layer 28 removed, constructional element 22, or crucible 38, is then removed from core 14.
Example 1
A heat-resistant self-supporting constructional element of zirconium silicate was prepared by plasma spraying a zirconium silicate powder having a particle size of about 0.040 to about 0.065 millimeters. The constructional element having an inner diameter of about 100 millimeters, an outside diameter of about 110 millimeters, and a length of about 960 millimeters was made by plasma spraying on the core an intermediate layer having a thickness of about 0.6 millimeters. Afterwards, the core was preheated to a temperature of about 400.degree. C., and the layer of zirconium silicate was deposited on the intermediate layer by plasma spraying. Immediately after finishing the plasma spraying operation, the core was severely cooled by water and separated from the self-supporting constructional element made of zirconium silicate.
Example 2
A heat-resistant self-supporting constructional element having an inner diameter of about 55 millimeters was prepared from a material based on aluminium oxide deposited by plasma spraying on an intermediate layer of aluminium having a thickness of about 0.3 millimeters. After cooling the core, the intermediate layer was separated by treating it with a 50% water solution of hydrochloric acid while simultaneously cooling the reaction vessel. After removing the core and intermediate layer, the self-supporting constructional element was washed with running water until the pH reached about 6.0 to about 7.0, and then the constructional element was dried at a temperature of about 50.degree. C. to about 80.degree. C.
Example 3
In the production of a heat-resistant crucible made of zirconium silicate, the intermediate layer was potassium chloride and was deposited by plasma spraying to a thickness of about 0.5 millimeters. After applying the zirconium silicate by plasma spraying, the intermediate layer was thereafter removed from the core by dissolving in water.
While this invention has been described as having a preferred embodiment, it will be understood that it is capable of further modifications. This application is therefore intended to cover any variations, uses, or adaptations of the invention following the general principles thereof, and including such departures from the present disclosure has come within known or customary practice in the art to which this invention pertains and fall within the limits of the appended claims.