Background of the Invention
The invention is related to a coating composition and in particular to a fluorocarbon polymer coating composition.
Fluorocarbon polymers are inert to strong acids such as sulfuric acid, nitric acid, hydrochloric acid and strong bases such as sodium hydroxide and are resistant weathering and salt water corrosion and are tough and abrasion resistant. Coatings of these polymers would be extremely useful for chemical plants and oil refineries to coat pipes, vessels and other equipment, for off shore oil well platforms and ships, and for protective coatings for the interior of smoke stacks of utility companies. Fluorocarbon polymer coatings also would be useful for coating metal smoke stack interiors that are subjected to abrasion from fly ash and corrosion by acids resulting from combustion products such as SO.sub.x and NO.sub.x and halogen ions. Conventional fluorocarbon polymer coatings require curing at elevated temperatures which is not possible with the aforementioned large structures. A fluorocarbon polymer coating composition is needed that can be applied as a thick coating without cracking and will completely cure at ambient temperatures.
The coating composition of this invention cures at ambient temperatures, has excellent adhesion to a variety of substrates, is corrosion and abrasion resistant and can be applied as a thick coating without cracking.
Summary of the Invention
A coating composition containing about 10-70% by weight binder and 30-90% by weight of a nonaqueous organic liquid, wherein the binder is
a fluorocarbon polymer in solution of vinylidene fluoride and hexafluoropropylene that has a weight average molecular weight of about 5,000-600,000;
dispersed fluorocarbon polymer particles of the following group: polytetrafluoroethylene, fluorinated/ethylene propylene polymer, polyvinyl fluoride, polyvinylidene fluoride and copolymer of tetrafluoroethylene/per fluoroalkoxyvinyl ether;
a metallic oxide such as magnesium oxide which is an acid acceptor; and
a curing agent of the formula ##STR1## where R is R.sup.1 NH.sub.2 and R.sup.1 is an aliphatic or cycloaliphatic hydrocarbon radical, R.sup.2 is C or a hydrocarbon group, R.sup.3 is H or CH.sub.3 and x is 3 when R.sup.2 is a hydrocarbon group and x is 4 when R.sup.2 is C;
Preferably, the composition contains a reinforcing pigment such as titanium dioxide.
Detailed Description of the Invention
The coating composition contains about 10-70% by weight binder and about 30-90% by weight of a nonaqueous organic liquid. The binder is a blend of a fluorocarbon polymer in solution, a dispersed fluorocarbon polymer, a metallic oxide which is an acid acceptor and a curing agent. An advantage of the composition is that it cures at ambient temperatures and baking is not required. Also, thick coatings of 1000 microns and greater can be applied without cracking of the coating during curing. Therefore, the composition can be used on large structures such as chemical storage tanks, chemical reactors, the interior of smoke stacks, and the like. These structures could not be subjected to baking temperatures using conventional techniques.
The fluorocarbon polymer that is in solution is of polymerized monomers of vinylidene fluoride and hexafluoropropylene. Preferably, the polymer contains about 50-70% by weight of vinylidene fluoride and about 30-50% by weight of hexafluoropropylene. The polymer can contain up to 40% by weight of other monomers such as tetrafluoroethylene. One useful polymer contains about 20-30% by weight of tetrafluoroethylene.
The fluorocarbon polymer has a weight average molecular weight of about 5,000-600,000. Preferably, fluorocarbon polymers are used that have a weight average molecular weight of about 75,000-450,000. Fluorocarbon polymers having a weight average molecular weight of 50,000-300,000 are useful. Two particularly useful fluorocarbon polymers have weight average molecular weight of about 75,000-125,000 and 150,000-250,000. Polymer in the lower end of the molecular weight range are preferred for forming a composition with higher binder content. Fluorocarbon polymers in the higher molecular weight range of 300,000-450,000 are also very useful for forming coating compositions.
Preferably, a soluble low molecular weight fluorocarbon polymer of vinylidene fluoride and hexafluoropropylene having a weight average molecular weight of about 5,000-15,000 is used in combination with a higher molecular weight fluorocarbon polymer. This low molecular weight polymer aids in dispersing pigments and the dispersed fluorocarbon polymer and forms films of 1000 microns and above without cracking of the coating on curing.
Molecular weight, as used therein, is determined by gel permeation chromatography using polymethyl methacrylate as a standard.
The dispersed fluorocarbon polymer used in the composition is not soluble in the organic liquid. Typical dispersed fluorocarbon polymers that can be used are polytetrafluoroethylene, fluorinated ethylene/propylene polymers preferably having a 70-30% by weight ethylene and 30-70% by weight propylene, polyvinylfluoride, polyvinylidene fluoride and copolymers or tetrafluoroethylene/perfluoro alkoxyvinyl ether preferably containing 8-98% by weight tetrafluoroethylene and 2-10% by weight perfluoroalkoxyvinyl ether. These dispersed fluorocarbon polymers usually have a particle size of about 1-150 microns.
These dispersed fluorocarbon polymers provided coatings with increased temperature resistance in comparison to coatings that do not contain dispersed fluorocarbon polymers. Also, coatings containing dispersed fluorocarbon polymers can be applied at a higher solids content which reduces solvent emissions. In general, the dispersed fluorocarbon polymer in the coating reinforces the coating and when the coating is subjected to temperatures which are sufficient to coalesce the dispersed fluorocarbon polymer, the polymer flows and coalesces into a matrix with the solution fluorocarbon polymer thereby enhancing physical properties of the coatings.
A metallic oxide which is an acid acceptor is used in the composition to react with the hydrofluoric acid which is generated during the curing or crosslinking reaction. Typical metallic oxides are magnesium oxide, lead oxide, calcium oxide, lead hydrogen phosphite and a mixture of calcium oxide and magnesium oxide. Magnesium oxide is preferred. Highly purified magnesium oxide is particularly preferred for high quality finishes.
The coating composition contains an amine curing agent of the formula ##STR2## where R is R.sup.1 NH.sub.2 and R.sup.1 is an aliphatic or cycloaliphatic hydrocarbon radical, R.sup.2 is C or a hydrocarbon group, R.sup.3 is H or CH.sub.3, X is 3 when R.sup.2 is a hydrocarbon group and X is 4 when R.sup.2 is C.
The curing agent is prepared through a Micheal's reaction in which a multifunctional acrylate or methacrylate is reacted with a polyamine. The polyamine is heated to about 100.degree.-150.degree. C. and then the multifunctional acrylate or methacrylate is reacted with the polyamine for a 1-6 hour period to form an amine terminated curing agent.
Typical polyamines used to form the curing agent are isophorone diamine which is 3-aminomethyl-3,5,5-trimethyl cyclohexylamine, hexamethylene diamine, ethylene diamine, 1,4-cyclohexane bis(methylamine), 1,2 diaminopropane, propylene diamine, diethyl ether diamine, trimethyl hexamethyl methylene diamine and the like.
Typical multifunctional acrylates or methacrylates that can be used to form the curing agent are trimethylol propane acrylate, trimethylol propane methacrylate, pentaerythritol acrylate, pentaerythritol methacrylate and the like.
Isophorone diamine is one preferred polyamine which is used to form a curing in which R is ##STR3##
Preferably, the binder contains about 50-84.5% by weight, of the solution fluorocarbon polymer 5-20% by weight of a low molecular weight fluorocarbon polymer, 5-20% by weight of dispersed fluorocarbon polymer 0.5-20% by weight of the above amine curing agent and 5-20% by weight of a metallic oxide which is an acid acceptor such as magnesium oxide.
Another useful binder contains about 50-89.5% by weight of the solution fluorocarbon polymer, 5-20% by weight of the dispersed fluorocarbon polymer 0.5-20% by weight of one of the above amine curing agents and 5-20% by weight of a metallic oxide which is an acid acceptor.
Preferably, the composition contains a reinforcing agent such as titanium dioxide pigment usually in a pigment to binder weight ratio of about 20:100 to 200:100. Other inert pigments can be used such as barytes, barium sulfate, fibrous calcium silicate and the like. Carbon black, bone black or lamp black can also be used as a reinforcing pigment in a pigment to binder weight ratio of about 20:100 to 50:100.
Typical organic solvents that are used in the composition are acetone, tetrahydrofuran, methyl ethyl ketone, ethyl acetate, propyl acetate, butyl acetate, isobutyl acetate, methyl isobutyl ketone, methyl amyl acetate, diisobotyl ketone, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether and mixtures of the above. These solvents are used to make the composition and can be used to reduce the composition to an application viscosity.
To decrease curing time and increase toughness of finishes of the composition about 0.1-3% by weight, based on the weight of the binder, of a bicyclic amidine can be added. One preferred bicyclic amidine is 1,8-diaza-bicyclo(5,4,0)-undecene-7.
To improve resistance to acids at ambient temperatures and elevated temperatures of finishes formed by the composition about 1-20% by weight, based on the weight of the binder, of a perfluoroalkyl propylene oxide can be added. The perfluoroalkyl propylene oxide has the formula ##STR4## where R.sup.4 is a perfluoroalkyl group having 4-12 carbon atoms. Preferably, R.sup.4 is a perfluoroalkyl group of a mixture of 6-10 carbon atoms. Preferably, about 5-15% by weight of the perfluoroalkylpropylene oxide is added.
Other advantages of the perfluoroalkylpropylene oxide are as follows: the surface tension of the coating is lowered and the resulting finish has improved release characteristics in comparison to finishes that do not contain the perfluoroalkylpropylene oxide; the wetting of pigments is improved and makes dispersion of pigments less difficult and fluorocarbon polymer solids of the composition can be increased.
A combination of the aforementioned bicyclic amidine and the perfluoroalkyl propylene oxide allows the removal of the metallic oxide from the coating composition and still provides a composition that cures at ambient temperatures. Generally, about 1-10% by weight, based on the weight of binder, of the combination is used. The weight ratio of bicyclic amidine to perfluoroalkylpropylene oxide is about 1:1 to 1:5.
To improve flow of the coating composition and enhance smoothness of the resulting finish about 1-20% by weight, based on the weight of binder, of a glycidyl ester can be added to the composition. Preferably, about 5-15% by weight of glycidyl ester is used. The ester has the formula ##STR5## where R.sup.5 is a tertiary aliphatic hydrocarbon group having 8-10 carbon atoms.
Generally, the composition is provided to a user as a two component composition. The solvents, solution fluorocarbon polymer, the dispersed fluorocarbon polymer, pigments such as titanium dioxide and metallic oxide acid acceptor are the first component and the amine curing agent is the second component which is blended by the user with the first component to form the coating composition. The composition is then reduced with one of the aforementioned solvents to an application viscosity and then applied to a substrate.
The coating composition can be applied directly over a wide variety of substrates to provide a fluorocarbon polymer coating. Typical substrates are treated or primed steel, phosphatized steel, grit blasted steel, galvanized steel, aluminum, copper, brass, cement and cementitious surfaces such as fire brick, mortar used for fire brick and the like.
Generally, the coating composition is spray applied to the substrate and the solvent is allowed to flash off between coatings, then the resulting coating is cured at ambient temperatures. The coating can be cured in about 4 to 48 hours or longer or can be heated to 80.degree. C. to 120.degree. C. for 0.5 to 2.0 hours for rapid curing. Generally, the resulting cured coating is about 75-1500 microns thick.
For some substrates such as untreated steel, a primer is first applied and then while the primer is still wet the coating composition is applied and dried at ambient temperatures or at the above elevated temperatures.
One useful primer contains the aforementioned binder constituents and the proper pigmentation for a primer. Another useful primer contains the solution fluorocarbon polymer, a metallic oxide acid acceptor such as magnesium oxide and amino alkyl alkoxy silane such as amino-propyl trimethoxysilane or amino-propyl triethoxysilane.
The ambient temperature curing characteristic of the coating composition allows for its application on large vessels and reactors in chemical plants and oil refineries, large metal structures and equipment and pipes, heat risers, i.e., pipes which are used to transport oil from the underground well to the surface, off shore oil well platforms, and on the interior or smoke stacks used by large utility companies. Conventional compositions that do not cure at ambient temperatures but require elevated temperatures are not practical to use for the above applications.
The following examples illustrate the invention. All parts and percentages are on a weight basis unless otherwise indicated.
Example 1
An amine curing agent was prepared as follows:
The diamine was charged into a reaction vessel and heated to about 120.degree.-140.degree. C. and then the acrylate was slowly added at a uniform rate over a 4 hour period and then the resulting reaction mixture was cooled and isopropanol was added.
A coating composition was prepared as follows:
The constituents of portion 1 were charged into a mixing vessel and thoroughly blended and portion 2 was added and blended. The resulting composition was reduced with methyl ethyl ketone solvent to a spray viscosity of about 25 seconds using a No. 2 Zahn cup and sprayed onto grit blasted steel panels and aluminum panels. In each case, thick films were applied by allowing flash drying between each application and the coatings were dried at ambient temperature to provide a 1000 micron thick dry coating. In each case, the coating had excellent adhesion to the metal substrate. After 7 days, the coatings were fully cured and resistant to sulfuric acid, sodium hydroxide and solvents such as methyl ethyl ketone and ethyl acetate.
A primer was prepared as follows:
The constituents of portion 1 were charged into a mixing vessel and thoroughly blended and then portion 2 was added and blended. The resulting composition was reduced to a spray viscosity with methyl ethyl ketone and sprayed onto untreated steel panels and solvent was allowed to flash from the primer at ambient temperatures. The resulting primer coat had a thickness of about 75 microns.
The above coating composition was sprayed onto the primed panels. In each case, thick films were applied by allowing flash drying between each spray application of the coating composition. The resulting coatings were dried at ambient temperatures and were 1000 microns thick.
On each panel, the coating had excellent adhesion to the primer and could not be separated from the primer. After 7 days, each coating was fully cured and was resistant to sulfuric acid, sodium hydroxide and solvents such as methyl ethyl ketone and ethyl acetate.
Example 2
The following amine curing agents were prepared:
In the preparation of each of the above curing agents A-C the amine was charged into a reaction vessel and heated to 120.degree.-140.degree. C. and then the acrylate was slowly added at a uniform rate over a 4 hour period and then the reaction mixture was cooled and isopropanol added.
Trimethylol propane acrylate and pentaerythritol acrylate were prepared by conventional techniques well known to those skilled in the art in which acrylate moiety was attached to trimethylol propane and pentaerythritol.
A separate coating composition was prepared with each of the curing agents A-C using the same constituents as in Example 1 for the coating composition except the above curing agent was substituted for the amine curing agent of Example 1. In each case, the resulting coating composition was reduced to a spray viscosity with methyl ethyl ketone as in Example 1 and sprayed onto grit blasted steel panels and aluminum panels allowing the coating to flash dry between each application to provide a 1000 micron thick dry coating. After 7 days, the coatings were fully cured but were softer and more elastic than the coating of Example 1. The coatings were resistant to sulfuric acid, sodium hydroxide and methyl ethyl ketone.
Example 3
Coating compositions 1-10 were prepared using the constituents shown in the attached Table. For each composition, the constituents of portion 1 were charged into a mixing vessel and thoroughly blended and portion 2 was added and blended. The resulting composition was reduced with methyl ethyl ketone solvent to a spray viscosity of about 25 seconds using a No. 2 Zahn cup and sprayed onto grit blasted steel panels and aluminum panels. In each case, thick films were applied by allowing flash drying between each application and the coatings were dried at ambient temperatures. The resulting dry coatings were a 1000 microns thick. In each case, the coatings from compositions 1-10 had excellent adhesion to the metal substrate. After 7 days, each of the coatings of compositions 1-10 were fully cured and were resistant to sulfuric acid, sodium hydroxide and solvents such as methyl ethyl ketone and ethyl acetate.
Example 4
Coating compositions 11-13 were prepared as follows:
For each coating composition Portion 1 was charged into a pebble mill and ground to a fineness of 0.5 mils. Portion 2 was then mixed with Portion 1 to form a coating composition. The resulting composition was reduced with methyl ethyl ketone to a spray viscosity of about 25 seconds using a No. 2 Zahn cup and sprayed onto grit blasted steel panels and aluminum panels. In each case, thick films were applied by allowing flash drying between each application and the coatings were dried at ambient temperatures. The resulting dry coatings were a 1000 microns thick. In each case, the coatings from compositions 11-13 had excellent adhesion to the metal substrate. After 7 days, each of the coatings of composition 11-13 were fully cured and were resistant to sulfuric acid, sodium hydroxide and solvents such as methyl ethyl ketone and ethyl acetate.