US 4,374,920 AGrant
Positive Developer Containing Non-Ionic Surfactants
Issue Date:1983-02-22
•8 Claims
Abstract
A developer composition for positive working lithographic printing plates and photoresists comprising an aqueous alkaline solution with a non-ionic surfactant.
Metadata
Assignee
- American Hoechst Corporation
Inventors
- Stanley F. Wanat
- Shane Hsieh
Application Information
Application Number:US 2874652
Filing Date:1981-07-27
Priority Date:1981-07-27
Art Unit:162
Classifications
IPC:
G03C 524
Field of Search:
430331;309
Patent Drawings
This patent does not have any drawings.
Description
Background of the Invention
The present invention relates to developer compositions for lithographic printing plates. More particularly, the invention relates to developers for printing plates of the so-called positive type which are sensitized with o-quinone diazide photosensitive materials.
It is known that the diazo groups of o-quinone diazides are removed by irradiation to actinic light, and that the compound itself changes to a compound with a carboxyl group. When the photosensitive coating containing o-quinone diazide is exposed to the light and developed with an alkaline developer, the part exposed to light is removed while the part not exposed to light remains as the image. Because of this characteristic, it is known as a positive-type photosensitive component for printing plates or for photoresist compositions. Compositions of o-quinone diazide are usually mixed with alkali-soluble resins having economical and practical advantages in such uses. Mixtures of phenol formaldehyde resins, or cresol formaldehyde resins, are generally used as the alkali soluble resins. Trisodium phosphate, sodium hydroxide, or sodium silicate alone, or their mixed aqueous solutions are used as a developer for sensitive films containing these o-quinone diazides. However, aqueous solutions of these developers tend to have detrimental etching effects on such printing plate substrate metals as aluminum. Also, the results of development vary considerably. In extreme cases, even a slight excess of developing time causes failure in image formation. If alkalinity is decreased, development speed decreases unacceptably. If alkalinity is increased, the aluminum or aluminum oxide substrate etches away, thus undesirably undermining and removing image as well as non-image areas.
Japanese Pat. No. 75-51324 suggests one method of attacking this problem. It teaches the addition of both an anionic and a dipolar surfactant to the aqueous alkaline developer solution.
Surfactants have also been used in other types of developers. U.S. Pat. No. 3,891,438 teaches the development of negative working printing plates sensitized by diazonium salts with aqueous solutions of organo-lithium salts to which anionic, cationic or non-ionic surfactants have been added.
Summary of the Invention
The present invention provides a developer solution for positive working photographic elements such as lithographic printing plates and photoresists which comprises an aqueous solution of hydroxide ions such as from an alkali and a compatible non-ionic surfactant.
This composition has been determined to substantially preserve the development speed as compared to an element developed with the alkali alone in solution and yet effectively, substantially acts as a barrier to the etching action of the aluminum.
Detailed Description of the Preferred Embodiment
As hereinbefore mentioned the developer of the present invention comprises an aqueous solution of an alkali and a compatible non-ionic surfactant.
Any composition capable of releasing hydroxide ions in solution is a suitable alkali useful for the practice of this invention. These include compounds which directly ionize in water or salts which generate hydroxide ions in water.
Non-limiting examples of alkalis useful for the practice of the present invention include sodium silicate, sodium metasilicate, trisodium phosphate, monosodium phosphate and sodium hydroxide.
Non-limiting examples of non-ionic surfactants useful for the practice of the present invention are those which are compatible with the alkali solution. That is, those which do not cause a precipitate when mixed with the aqueous alkali solution. Examples include ethoxylated phenols, tetramethyl decynediol, ethoxylated tetramethyl decynediol, ethoxylated aliphatic alcohols, alkylene oxide block copolymers, fatty acid amides, and ethoxylated diols. Especially preferred surfactants include Triton X-100 available from Rohm & Haas of Philadelphia, Pa; Tergitol Min Foam 1x available from Union Carbide Corporation; Antarox BL-330 available from GAF and Amidox C-5 available from Stepan Chemical Co. of Northfield, Ill.
Other preferred surfactants are the Surfynols available from Air Products and Chemicals, Inc. of Allentown, Pa. These generally have the formula ##STR1## where R=methyl
R'=isobutyl
R"=OH or (--O--CH.sub.2 --CH.sub.2).sub.x --OH
These surfactants are believed to act as a barrier to aluminum etching while maintaining the speed of the aqueous alkaline developer.
Commonly, salts are used in addition to the source of hydroxide ions. These are capable of forming hydrophilic water-insoluble coatings on the metal, produce alkaline-reacting systems themselves in water or help buffer the system. These may be present in the range of 0.2-10% by weight with the preferred salt content in the range of 0.5-5% by weight.
Representative of these salts are the following in aqueous alkaline solution:
salts of hydrofluosilicic acid M.sup.I.sub.2 (SiF.sub.6) and M.sup.II (SiF.sub.6)
salts of hydrofluotitanic acid M.sup.II (TiF.sub.6) and M.sup.III (TiF.sub.6)
salts of hydrofluostannic acid M.sup.I (SnF.sub.6)
salts of hydrofluoboric acid M.sup.I (BF.sub.6)
salts of orthosilicic acid or metasilicic acid M.sup.I O.xSiO.sub.2.xH.sub.2 O
salts of orthotitanic acid 2M.sup.I.sub.2 O.TiO.sub.2 and
salts of stannic acid M.sup.I (Sn(OH).sub.6)
wherein M is a metal ion. These salts are more fully described in U.S. Pat. No. 3,110,596 which is incorporated herein by reference.
In the preferred embodiment, the alkali may be present in the developer in an amount of from about 0.2 to about 12 parts by weight; more preferably 0.2 to about 10; most preferably 3 to about 8.
In the preferred embodiment, the non-ionic surfactant may be present in the developer of the present invention in an amount of from about 0.1% to about 10% by weight; more preferably 0.5 to 3% by weight of the developer.
The pH of the developers of this invention generally range from about above 7.0 to about 14, more preferably about 11 to about 13.
Preferred developer formulations comprise the Triton X-100 surfactant in any of the following developers:
The following non-limiting examples demonstrate the invention.
Example 1
5.times.7" samples of P-150 (positive printing plates available from the Azoplate Division of American Hoechst Corporation, Branchburg, N.J.) are exposed in a vacuum frame for a fixed number of time units (30 secs. e.g.). In a small tray .about.750 ml. of positive developer is used to develop a plate. The tray is rocked on a rocker attached to a timer. The developer composition may be as follows:
Development is fixed at 15 minutes. The plate is rinsed and blotted dry. This is a control sample. Sample plates are then successively developed in a similar fashion with 7.5 ml. (1%) of the surfactant under study. plates are rinsed and dried and compared to the control. Table 1 demonstrates the results effected with several surfactant types.
Comparison is based on (1) Stauffer 21 step scale (a higher clear step indicates more aggressive development. (2) Half tone dot sharpening (reduction) or loss. (3) Attack of non-image area oxide as well as the intermediate steps of the Stauffer scale, as evidenced by formation of a white powdery oxide which can be wiped off readily.
Example 2
The procedure of Example 1 may be repeated using the following developer:
Since this is a more aggressive developer, the samples are rock developed for only 7 mins. All other aspects of the procedure were similar. The following results are noticed when the indicated surfactant is added at 1% by weight.
Claims
What is claimed is:
1. A developer for positive working photographic elements which comprises an aqueous solution of hydroxide ions having a pH above about 7.0 provided from an alkali having a concentration in the developer which ranges from about 0.2 to about 10 percent by weight; and a compatible non-ionic surfactant selected from the group consisting of one or more of tetramethyl decynediol and ethoxylated tetramethyl decynediol.
2. The developer of claim 1 further comprising one or more compounds selected from the group consisting of the metal salts of hydrofluosilicic acid, hydrofluotitanic acid, hydrofluostannic acid, hydrofluoboric acid, orthosilicic acid, metasilicic acid, orthotitanic acid and stannic acid.
3. The developer of claim 2 wherein the concentration of alkali ranges from about 0.2 to about 10 percent by weight.
4. The developer of claim 3 wherein the concentration of surfactant ranges from about 0.1 to about 10 percent by weight.
5. The developer of claim 1 wherein the concentration of surfactant ranges from about 0.1 to about 10 percent by weight.
6. A developer for positive working photographic elements which comprises an aqueous solution of hydroxide ions having a pH above about 7.0 from an alkali selected from the group consisting of one or more of trisodium phosphate, sodium hydroxide, monosodium phosphate, sodium silicate, and sodium metasilicate; and a compatible non-ionic surfactant selected from the group consisting of one or more of tetramethyl decynediol and ethoxylated tetramethyl decynediol.
7. The developer of claim 6 wherein the concentration of surfactant ranges from about 0.1 to about 10 percent by weight.
8. The developer of claim 6 further comprising one or more compounds selected from the group consisting of the metal salts of hydrofluosilicic acid, hydrofluotitanic acid, hydrofluostannic acid, hydrofluoboric acid, orthosilicic acid, metasilicic acid, orthotitanic acid and stannic acid.
Patent Citations (13)
| Patent | Date | Inventor | Cited By |
|---|---|---|---|
| US3110596 | 1963-11-01 | Heiss et al. | |
| US3586504 | 1971-06-01 | Coates et al. | |
| US3669660 | 1972-06-01 | Golda et al. | |
| US3707373 | 1972-12-01 | Martinson et al. | |
| US3738850 | 1973-06-01 | Radell et al. | |
| US3745028 | 1973-07-01 | Rauner | |
| US3868254 | 1975-02-01 | Wemmers | |
| US3891438 | 1975-06-01 | Katz | |
| US3891439 | 1975-06-01 | Katz et al. | |
| US3954472 | 1976-05-01 | Walls | |
| US4130425 | 1978-12-01 | Boyd | |
| US4308340 | 1981-12-01 | Walls | |
| JPX50-51324 | 1975-05-01 |
Non-Patent Literature (5)
- Schick, "Non-Ionic Surfactants," Marcel Dekker, Inc., N.Y., c 1967, pp. 413-414.
- Chemical Abstracts, 186365q Presensitized Photolithographic Printing Plates, Wade, John E., vol. 83, 1975, p. 491.
- Chemical Abstracts, 99071j Liquid Developers for Lithographic Photosensitive Plates Containing Diazo Compound, Matsumoto, Hiroshi, vol. 86, 1977, p. 649.
- Chemical Abstracts, 44133x Developers for Diazo-Sensitized Lithographic Plates, Rowe, William, vol. 81, 1974.
- Chemical Abstracts, 170917k Developer for Photosensitive Lithographic Plates Containing o-Quinonediazide Compounds, Watanabe, Masaru, vol. 83, 1975, p. 458.