This invention relates to cellular, intumescent materials and especially to materials which are substantially open-celled and which have been partially or wholly impregnated with a flexible, intumescent polymeric material.
U.K. Patent Specification No. 1,463,069 describes the production of an intumescent polyester-based urethane foam by incorporating an intumescent additive into the foamforming reaction mixture.
U.K. Patent Specification No. 1,519,795 describes the impregnation of an already-produced polyether-based urethane foam with a suspension or dispersion of a particular flame-retardant material.
Attempts to make an intumescent polyether-based urethane foam according to Specification No. 1,463,069 have not proved successful; it is believed that this lack of success is due, in part, to the fact that polyetherurethane molecules are less oxidised than polyesterurethane molecules, so that the former are much more liable to rupture than the latter on exposure to heat and/or fire.
If recourse is had to the method described in Specification No. 1,519,795, care must be taken to keep the amount of particulate material deposited within fairly close limits if the physical properties of the foam (e g compression set, resilience and flex-fatigue) are not to be unduly affected.
It has now been found that a normally-flammable, substantially open-celled, cellular material can be post-treated with an intumescent material so that the open-celled nature is essentially retained and that the treated material will intumesce and char in a fire situation.
Accordingly, the present invention provides a cellular, intumescent material consisting essentially of an open-celled substrate which has been at least partially impregnated with a flexible, intumescent polymeric material, whereby the open-celled nature of the material is retained and the said material will intumesce and char on exposure to a flame.
The cellular material may be a polyether-based urethane foam, a latex foam, a natural or a synthetic rubber, polybutadiene or a styrene/butadiene rubber. Impregnation of the cellular material may be performed by dipping, spraying or application from a dispenser followed by passing the material through the nip of a pair of rollers.
The flexible, intumescent polymeric material must comprise at least the following ingredients:
The binder may contain one or more cross-linking agents.
It is believed that an intumescent cellular material obtained according to the present invention is formed by the following reaction mechanism.
(a) the polyhydric material and the acid/acid generator react to form an ester. This step may be assisted by the use of Catalyst C (above);
(b) the ester dehydrates, leaving a carbon-rich substrate;
(c) gases evolved (with, if present, the assistance of Blowing Agent F) cause the carbon-rich substrate to foam.
During events (a) and (b) above, the reaction mixture melts. The release of gas, either as water from the dehydration stage or from the blowing agent, causes the melt to puff and foam. Finally, the molten mass solidifies to give a foamed carbonaceous char which forms a heat-insulative barrier.
Thus, the normally-flammable cellular material is surrounded by an intumescent foam layer.
Treatment of cellular materials according to the present invention permits polyether-based urethane foams to be used in situations where there is a risk of exposure to heat and/or fire. Polyether-based urethane foams, when compared with polyester-based foams, show better dynamic properties (especially compression-set) and better hydrolytic properties, in addition to being less costly to produce.
The present invention will be illustrated by way of the following Examples.
Example I
The ingredients shown in TABLE A (below) were mixed together.
The mixture was sprayed on to the surface of a block of polyether-based urethane foam (Dunlopillo DI grade-available from Dunlop Limited) to give a surface covering of weight 500 g/m.sup.2 and a penetration depth of about 3 mm.
On exposure of the treated foam to a "roaring" Bunsen flame (temperature about 900.degree. C.) the foam surface intumesced and charred. On removal of the flame, afterburning of the foam extinguished in 2 to 3 seconds.
Example Ii
The mixture described in Example I (above) was used to impregnate a block of 80:20 SBR/NR latex foam to a depth of 3 mm, giving a surface covering of weight 1169 g/m.sup.2.
On exposure of the treated foam to a "roaring" Bunsen flame the foam surface intumesced and charred. On removal of the flame, after-burning of the foam extinguished in 5 to 6 seconds with the inner core of the foam smouldering slowly. An untreated sample burnt fiercely and completely.
Example Iii
To a 10% solution of an isoprene-based thermoplastic rubber (available as CARIFLEX* TR-1107) in toluene there was added sufficient para-nitroaniline bisulphate to make a 1:2 dispersion. This dispersion was used to impregnate a block of polyether-based urethane foam (Dunlopillo Dl) to give a surface covering of weight 614 g/m.sup.2 and a penetration depth of 3 mm.
On exposure of the treated foam to a "roaring" Bunsen flame the foam surface intumesced and charred. On removal of the flame, after-burning of the foam extinguished in 5 to 6 seconds.
Example Iv
A block of Dunlopillo D-10 flexible polyurethane foam, having dimensions of 15.times.15.times.4 inches and a density of 30 Kg/m.sup.3, was impregnated with a dispersion of an intumescent composition in a neoprene latex, the composition being made from the ingredients shown in TABLE B (below).
The impregnated foam was placed in an oven at 110.degree. C. in order to remove the water and cure the binder. The foam was removed from the oven when constant weight had been achieved.
On exposing a small sample of the impregnated foam to a roaring Bunsen flame it flamed initially and then formed a protective char approximately 3 mm thick and extinguished.
The block of foam was covered with a sheet of cotton which had been treated with a commercially-available flame-retardant material, believed to consist essentially of the reaction product of tetrakishydroxymethyl phosphonium chloride and ammonia, available from Albright and Wilson Ltd as PROBAN (Registered Trade Mark).
Two wooden cribs, each containing wood-wool in the centre was placed centrally on top of the cotton cover. Each crib was made up as follows:
The sticks in each layer were placed as far away from each other as possible (but without any overhang) and glued together with a small amount of PVA adhesive. The ignition source was conditioned in an atmosphere having a temperature of 20.degree..+-.2.degree. C. and a relative humidity of 65%.+-.5% for at least 16 hours before testing and the test undertaken within 1 hour after removal from the conditioning area.
When ignited the cribs burnt for 41/2 minutes. All signs of flaming had ceased after 7 minutes and no smouldering was occurring. On examination the foam sample exhibited a crater some 8" in diameter and 2" in depth lined with a black char which had intumesced in patches.