US 4,265,976 AGrant
Radiation-Curable Coated Article Having Moisture Barrier Propetes
Issue Date:1981-05-05
•5 Claims
Abstract
This invention provides an ultraviolet radiation-curable coating composition which after curing has utility as a moisture barrier film for the protection of substrates such as paper and cardboard. Illustrative of the invention radiation-curable composition is a blend of components comprising (1) chlorinated rubber, (2) chlorinated paraffin; (3) vinyl acetate; (4) trimethylolpropane triacrylate; (5) photoinitiator; and (6) heat and light stabilizer for the chlorocarbon components. The invention composition cures as a substantially 100 percent solids system within one second at room temperature when exposed to ultraviolet radiation.
Metadata
Assignee
- Celanese Corporation
Inventor
- Michael T. Nowak
Application Information
Application Number:US 076020&
Filing Date:1979-09-17
Priority Date:1978-09-19
Art Unit:164
Classifications
IPC:
B32B 904
Field of Search:
428204427486;512;485;487;513;496159.1754.1
Patent Drawings
This patent does not have any drawings.
Description
The following examples are further illustrative of the present invention. The reactants and other specific ingredients are presented as being typical, and various modifications can be devised in view of the foregoing disclosure within the scope of the invention.
Example I
This Example illustrates the preparation of a preferred radiation-curable resin composition in accordance with the present invention.
The following ingredients were blended at room temperature with stirring.
The curable resin composition had a pot stability greater than two weeks at 120.degree. F.
A 0.2 mil coating on detergent box stock cured in 0.1 seconds when exposed to a mercury vapor lamp of 200 watts per linear inch power, at a distance of 12 inches.
The rate of water vapor penetration through a 0.2 mil coating as measured by a Honeywell Moisture Barrier Tester was 1.3 grams/100 square inches/24 hours.
Example Ii
This Example illustrates moisture barrier test results of a present invention ultraviolet cured invention coating in comparison with other coating systems.
The results in Tables I and II demonstrates that the moisture-barrier properties of a present invention coating are enhanced by a synergistic interaction between the chlorinated rubber and chlorinated paraffin components of the coating system.
Claims
What is claimed is:
1. An article comprising a substrate in combination with an adherent moisture barrier protective film, which combination is produced by coating the substrate surface with a resin composition, and then radiation-curing the said coating to form the moisture barrier protective film on the substrate surface; wherein the resin composition comprises a blend of (1) between about 10 and 30 weight percent of chlorinated rubber; (2) between about 2 and 25 weight percent of chlorinated paraffin; (3) between about 15 and 45 weight percent of vinyl alkanoate; (4) between about 10 and 40 weight percent of crosslinking monomer containing at least two polymerizable olefinically unsaturated groups; (5) between about 0.5 and 15 weight percent of photoinitiator; and (6) between about 0.5 and 5 weight percent of stabilizer, based on the total composition weight.
2. An article in accordance with claim 1 wherein the substrate is a flexible cellulosic sheet composition.
3. An article comprising a substrate in combination with an adherent moisture barrier protective film, which combination is produced by coating the substrate surface with a resin composition, and then ultraviolet radiation-curing the said coating to form the moisture barrier protective film on the substrate surface; wherein the resin composition comprises a blend of (1) between about 15 and 25 weight percent of chlorinated rubber; (2) between about 5 and 20 weight percent of chlorinated paraffin; (3) between about 20 and 35 weight percent vinyl acetate; (4) between about 15 and 35 weight percent of crosslinking monomer selected from trimethylolpropane triacrylate and trimethylolpropane trimethacrylate; (5) between about 1 and 10 weight percent of photoinitiator; and (6) between about 1 and 4 weight percent of heat and light stabilizer for the chlorocarbon components, all based on the total composition weight.
4. An article in accordance with claim 3 wherein the substrate is a flexible sheet of paper or cardboard.
5. An article in accordance with claim 3 wherein the moisture barrier protective film on the substrate surface exhibits a rate of water vapor transmission of less than 2 grams/100 square inches/24 hours at a film thickness of about 0.2 mil.