Background of the Invention
The present invention relates to a process for the preparation of non-sticky particles containing a high concentration of a highly viscous substance. More particularly, the invention relates to a process for preparing, by granulation, non-sticky particles containing a high concentration of a viscous substance selected from the group consisting of higher alcohols having 8 to 18 carbon atoms and which are soft or molten or liquid at a temperature lower than 40.degree. C. and non-ionic surface active agents having the following formulae (I) and (II): ##STR2## and
wherein R.sub.1 is alkyl having 4 to 18 carbon atoms, R.sub.2 is alkyl or alkenyl having 8 to 22 carbon atoms, and n and m each is a number of from 1 to 50.
Description of the Prior Art
As means for granulating the viscous substances mentioned above, there is known a method which comprises adding to the viscous substance a fine powder of an inorganic substance such as aluminum hydroxide, talc or the like. In particles prepared by this known method, however, it is difficult to prevent cohesion and caking of the particles during storage, and the concentration of the viscous substance has to be reduced to 20 weight % at most, usually 10 weight % or lower. Of course, if the desired property of solubility or dispersibility in water is sacrificed, it is possible to increase the concentration of the viscous substance to a level approximating 40 weight %. In this case, however, particles having a practical utility cannot be obtained.
For example, Japanese Patent Publication No. 25630/65 discloses a method in which a water-insoluble synthetic resin film is formed on the viscous substance. According to this method, however, since attainment of improvements of moisture resistance and water resistance is intended, even if caking is prevented, the resulting particles cannot be applied to use in aqueous systems.
Further, Japanese Patent Publication No. 25317/64 discloses a process for preventing caking by treating surfaces of particles with non-sticky fine powder. According to this process, the non-sticky fine powder should be employed in a large quantity if a viscous substance such as those mentioned above is treated.
Summary of the Invention
We have discovered a process for preparing a granulated product which is free of a tendency to cake and which contains at least 20 weight % of a viscous substance such as those mentioned above, without sacrifice of the water solubility or dispersibility thereof.
More specifically, in accordance with the present invention, there is provided a process for the preparation of granules containing a high concentration of a viscous substance, which granules are free-flowing and not apt to cake or agglomerate under normal storage conditions at ambient temperatures and ambient humidity conditions. According to the invention, there are incorporated in at least one viscous substance selected from the group consisting of higher alcohols having 8 to 18 carbon atoms and which are soft or molten or liquid at a temperature lower than 40.degree. C. and non-ionic surfactants having the foregoing formulae (I) and (II), (A) about 40 to about 300 weight %, based on the weight of said viscous substance, of an organic or inorganic compound capable of catching rapidly water of crystallization to form porous particles or of adsorbing physically water to form superficially porous particles, and (B) about 30 to about 100 weight %, based on the weight of said viscous substance, of an inorganic substance having a high affinity with said viscous substance and an effect of controlling the flowability of said viscous substance, then adding to the resulting mixture, (C) an aqueous solution of an inorganic or organic compound that is adhesive to substance (A), said solution containing water in an amount sufficient to impart at least one mole of water of crystallization or saturated water of adsorption to the substance (A), kneading the mixture to make it homogeneous and then granulating the kneaded mixture.
As the alcohol according to this invention, there is preferred an alcohol having the formula ROH wherein R is an acyclic saturated or ethylenically unsaturated hydrocarbon group having 8 to 18 carbon atoms.
As is seen from the foregoing description, the main substances to be added to the viscous substance, according to the process of the present invention, are the following three substances:
(A) An organic or inorganic substance capable of catching rapidly water of crystallization to form porous particles of hydrated salts or of adsorbing physically water to form apparently porous articles, which substance (A) includes, for example, inorganic compounds such as anhydrous sodium sulfate, anhydrous sodium tripolyphosphate, talc, bentonite and anhydrous calcium sulfate, and organic compounds water-insoluble cellulosic pulp and water-soluble cellulosic pulp such as hydroxyethyl cellulose and carboxymethyl cellulose.
(B) Fine powder of an inorganic compound having a high affinity with the viscous substance, a high absorbing property to the viscous substance and an effect of controlling the flowability of the viscous substance, which includes, for example, anhydrous silicic acid, aluminum silicate, magnesium silicate, calcium silicate, zeolites and aluminum hydroxide.
(C) An aqueous solution of an organic or inorganic compound capable of acting as an adhesive to the substance (A) while imparting water of crystallization or physically adsorbed water to the substance (A), which includes for example, aqueous solutions of sodium silicate, colloidal silica, colloidal aluminum, polyvinyl alcohol, sodium carboxymethyl cellulose and polyethylene glycol (having a molecular weight of at least 3,000).
The amount used of the substance (A) is about 40 to about 300 weight %, based on the weight of the viscous substance.
The amount used of the substance (B) is about 30 to about 100 weight %, based on the weight of the viscous substance.
The amount used of the substance (C) is such that water of crystallization is imparted to the substance (A) in an amount necessary for forming from a monohydrate to the maximum extent of hydration of the substance (A), or the substance (A) contains a maximum saturation amount of physically adsorbed water. An amount of the substance (C) to be added is preferred to range from 0.1 to 0.5 wt.% in the form of its aqueous solution having a concentration of 1 to 50 wt.%.
In order for the substance (A) to catch water of crystallization with ease and to form more porous cross-linked particles, it is preferred that the particle size of substance (A) is smaller than 60 mesh.
In order to control the flowability of the viscous substance sufficiently, it is preferred that the surface area of the substance (B) be large, namely, the particle size of substance (B) should be smaller than 30 microns.
According to the process of the present invention, the substance (B) is added to the viscous substance to control the flowability of the viscous substance, and then, the substance (A) is added to the mixture and the mixture is sufficiently blended and kneaded to form a homogeneous mixture. Then, the substance (C) is added in a total amount calculated so that the substance (A) comes to contain water in an amount necessary to transform (A) into porous particles. Substance C is gradually blended in the mixture over a period of 30 to 40 minutes while cooling the mixture with water or air, whereby the water in the substance (C) is caught in the substance (A) as water of crystallization, or physically adsorbed water, and porous particles are formed and simultaneously, the viscous substance having a reduced flowability is included in the voids of the thus-formed porous particles of (A).
The thus-obtained porous particles are granulated into larger particles by an extruding or rotary granulator. Thus, the viscous substance can be contained in the granulated product in an amount of 20 to 50 weight %, and a granulated product free of a tendency to cake and having a good water dispersibility can be obtained.
When the speed of forming cross-linked particles of (A) by inclusion of water of crystallization is too high, violent heat generation takes place and large agglomerates are readily formed. Further, it becomes difficult to include the viscous substance in the porous particles. Accordingly, the reaction of the water with (A) should be advanced gradually by suitably controlling the rate of addition of the aqueous solution of substance (C) so that no caking or agglomeration of (A) occurs.
The present invention will now be further described in more detail by reference to the following illustrative Examples.
Example 1
Polyoxyethylene (17) alkyl (C18) ether as the viscous substance was sufficiently mixed with anhydrous sodium tripolyphosphate and anhydrous silicic acid in a mixer, and then, an aqueous solution of diatomaceous earth No. 3 was added to the mixture.
Water in the aqueous solution of the diatomaceous earth No. 3 became included in anhydrous sodium tripolyphosphate as water of crystallization and heat was gradually generated. The entire mixture was gradually plasticized and partial granulation was initiated. The mixture was granulated by an extruding granulator to obtain a granulated product having a size of 12 to 48 mesh (JIS).
Example 2
Polyoxyethylene (9) secondary alkyl (C14) ether was sufficiently mixed with calcium silicate, and anhydrous sodium tripolyphosphate was added thereto. Mixing was further continued and the aqueous solution of polyvinyl alcohol was gradually added. The anhydrous sodium tripolyphosphate caught the water of the aqueous solution as water of crystallization and heat was generated. Thus, cross-linked porous particles were formed, and solidification was initiated in the particles containing as inclusions therein the polyoxyethylene (9) secondary alkyl (C14) ether as the viscous substance. Then, the particles were broken and granulated into a size of 12 to 48 mesh (JIS).
Example 3
Crystalline cellulose and aluminum silicate were blended in oleyl alcohol, and anhydrous sodium sulfate was added and the mixture was sufficiently agitated. When the aqueous solution of polyethylene glycol was added to the mixture, the anhydrous sodium sulfate caught the water of the aqueous solution as water of crystallization to form cross-linked particles. The particles were granulated to a size of 12 to 48 mesh (JIS) by a rotary granulator.
Example 4
All the components were mixed simultaneously and on completion of the mixing, the mixture was formed into granules having a size of 12 to 48 mesh.
Comparative Example 1
A mixture having the above composition was blended by agitation and formed into granules having a size of 12 to 48 mesh (JIS). The granulated product was dried at 60.degree. C. for 1 hour.
Comparative Example 2
A mixture having the above composition was blended by agitation and granulated into a size of 12 to 48 mesh (JIS). The granulated product was dried at 60.degree. C. for 1 hour.
Comparative Example 3
A mixture having the above composition was blended by agitation and granulated into a size of 12 to 48 mesh.