US 4,256,858 AGrant
Process for Cross-Linking Polymers Containing Active Halogen
Issue Date:1981-03-17
•6 Claims
Abstract
Process for cross-linking polymers which contain an active halogen by using a compound of the formulae: ##STR1## as a cross-linking agent.
Metadata
Assignee
- Bayer Aktiengesellschaft
Inventor
- Sigurd Behr
Application Information
Application Number:US 0608319
Filing Date:1979-07-25
Priority Date:1978-07-27
Art Unit:144
Classifications
IPC:
C08F 830
Field of Search:
525375;349
Patent Drawings
This patent does not have any drawings.
Description
This invention relates to a process for cross-linking polymers containing active halogen using certain products which make the polymers safer to process and which do not bring about an increase in the vulcanisation time.
Conventional cross-linking agents, for example for polychloroprene, are attended by the disadvantage that, on completion of the main reaction, cross-linking continues at a reduced velocity. This is reflected in the corresponding Vulkameter curves. It is no longer possible to speak in terms of post-cross-linking when, on completion of the main cross-linking reaction, the Vulkameter curve runs parallel to the time axis. If, however, the curve continues to climb, this is indicative of post-cross-linking. The difference in time between 90% and 80% vulcanisation (T.sub.90 -T.sub.80) may be regarded as a measure of post-cross-linking. If this difference is small, only minimal post-cross-linking occurs.
Technologically, post-cross-linking means that vulcanisates of large volume do not show a uniform degree of cross-linking or modulus over the cross-section thereof. This has an adverse effect inter alia in the event of dynamic stressing.
In addition, conventional cross-linking agents for polychloroprene bring about a cross-linking reaction which begins quickly, but continues slowly. This may also be seen from the Vulkameter curves. The incubation time (the time required to reach 10% vulcanisation) is short, whilst the cure time (the time required to reach 80% vulcanisation) is long, in other words the rise of the Vulkameter curve begins early and is relatively flat. In such a cross-linking reaction, the quotient T.sub.10 /T.sub.80 is small. Technologically, this is equivalent to a minimal level of safety in processing.
It has now been found that, where certain products are used, cross-linking is virtually completed with the main reaction and, with continued application of heat, no cross-linking occurs. It has also been found that the quotient T.sub.10 /T.sub.80 is considerably greater than, for example, where the conventional cross-linking agent, thiourea, is used. In addition the incubation time (T.sub.10) is surprisingly longer. It has also been found that the compounds used in accordance with the present invention provide for improved behaviour under dynamic flexural stressing by comparison with cross-linking carried out using thiourea.
Accordingly, the present invention relates to a process for cross-linking polymers containing active halogen which is characterised in that the cross-linking agents used are compounds corresponding to the following general formulae: ##STR2## wherein R.sub.1 represents hydrogen or, C.sub.1 -C.sub.4 alkyl;
R.sub.2 represents hydrogen, C.sub.1 -C.sub.14 alkyl, C.sub.1 -C.sub.14 alkoxy, C.sub.1 -C.sub.14 alkyl phenyl, phenyl, naphthyl, hydroxyl or, C.sub.1 -C.sub.14 alkyl hydroxyl;
R.sub.3 and R.sub.4, which may be the same or different, each represents hydrogen or, C.sub.1 -C.sub.4 alkyl;
R.sub.5 represents hydrogen or, C.sub.1 -C.sub.4 alkyl; and
R.sub.6 and R.sub.7, which may be the same or different, each represents hydrogen or C.sub.1 -C.sub.4 alkyl;
and in that cross-linking is carried out in the conventional way.
In the above general formulae, R.sub.2 preferably represents hydrogen, C.sub.1 -C.sub.14 alkyl, C.sub.1 -C.sub.4 alkoxy and phenyl.
Particularly preferred compounds are: isoquinoline, 9H-carbazol-2-ol, dimethyl acridane, quinoline and its 4- and 6-methyl derivatives, 1H-indole and its 2-methyl and 2,3,5-trimethyl derivatives, 2,2,4-trimethyl-1,2-dihydro-quinoline and its 5-,6-,7- or 8-methyl derivatives, its 6-ethoxy or 6-dodecyl or 6-phenyl derivatives, a compound corresponding to general formula (6) wherein R.sub.1, R.sub.3 and R.sub.4 each represents hydrogen or methyl and R.sub.2 represents hydrogen, a compound corresponding to general formula (7) wherein R.sub.2 and R.sub.5 each represents hydrogen and a compound corresponding to general formula (8) wherein R.sub.2, R.sub.3 and R.sub.4 each represents hydrogen. Other preferred compounds are the oligomers (degree of oligomerisation from 2 to 15) of the above-mentioned 1,2-dihydroquinoline.
Particularly suitable compounds are 2,2,4-trimethyl-1,2-dihydroquinoline or oligomers thereof, 6-methyl-,6-ethoxy-,6-dodecyl-or 6-phenyl-2,2,4-trimethyl-1,2-dihydroquinoline or oligomers thereof. (2,2,4-trimethyl-1,2-dihydroquinoline is referred to herein as TMDHCH.)
The compounds are known from the literature.
In the case of TMDHCH, for example, it was found that the level of reactivity during the cross-linking reaction is dependent upon the degree of oligomerisation (cf. Example 15). Accordingly, the cross-linking reaction may be controlled by selecting the degree of oligomerisation or by simultaneously using different degrees of oligomerisation.
Preferred polymers containing active halogen are halogen-containing diene rubbers, such as chlorinated polyisoprene, chlorinated or brominated natural rubber, chlorobutyl and bromobutyl rubber and also most preferably polychloroprene. These polymers are distinguished by the fact that they contain a reactive halogen atom.
Polymers of chloroprene unmodified or modified with sulphur, or mixtures thereof, may be used as the polychloroprene. In addition, it is possible to use copolymers which contain up to 50% of a compound copolymerisable with chloroprene, such as monovinyl compounds (acrylonitrile, methacrylonitrile, vinylidene chloride, .alpha.-chloroacrylonitrile, methacrylic acid esters and acrylic acid esters), vinyl-substituted aromatic compounds (styrene and vinyl toluenes) and conjugated diene compounds (1,3-butadiene,1-chloro-1,3-butadiene, 2,3-dichloro-1,3-butadiene, and 2-chloro-3-methyl-1,3-butadiene).
Where compounds corresponding to the above general formulae, preferably TMDHCH and, better still, in oligomeric form having a melting point of approximately 70.degree. C., are used, it has been found that, on the one hand, technically useful cross-linking, preferably in the case of polychloroprene, is obtained at room temperature (RT) or at a slightly elevated temperature whilst, on the other hand, the mixtures show a degree of safety in processing which, in the case of conventional polychloroprene accelerator systems, is only achieved by dispensing with self-vulcanisation. In addition, despite a long incubation time, there is no increase in the vulcanisation time at room temperature and slightly elevated temperature (cf. Example 9).
This enables rubber articles to be produced by processes which would otherwise have been unworkable. In many cases, this method of cross-linking at room temperature or a slightly elevated temperature eliminates the need for expensive, energy-consuming vulcanisation apparatus. Such vulcanisation apparatus is essentially required not only for supplying energy, but also for applying an external pressure to eliminate porosity in the vulcanisate.
There is no need for particular formulation-related measures, such as the addition of water binding agents, which in turn adversely affect the properties of the vulcanisates, because cross-linking at room temperature and at slightly elevated temperatures remains well below the boiling point of water. Similarly, there is frequently no need to use a vacuum extruder because at room temperature and at slightly elevated temperatures other readily volatile constituents of the mixture do not give rise to pore formation.
Vulcanisation apparatus may be utilised much more effectively insofar as it is only a shaping or forming pre-cross-linking reaction which is allowed to take place and further cross-linking is carried out at room temperature or a slightly elevated temperature by self-vulcanisation using the new cross-linking system (Examples 10, 11 and 12).
The compounds used according to the present invention, preferably the oligomeric TMDHCH, may also be used for cross-linking adhesive films, preferably based on polychloroprene. In this case, it has surprisingly been found that, despite the addition of the so-called "cross-linking agent" which, hitherto, has generally been an isocyanate, the so-called "pot life" is very considerably increased or is unaffected. Those skilled in the art know that, with isocyanates, pot life only amounts to a few hours. According to the present invention, there was no change in the viscosity of the polychloroprene adhesive solution after 20 days (Example 13).
It may be concluded from this that no cross-linking reaction takes place as long as solvents are present.
The new cross-linking systems may also be used in the latex field. Thus, it has been found that preferably TMDHCH (melting point approximately 70.degree. C.) cross-links a cast polychloroprene latex film both at normal vulcanisation temperatures and also at room temperature and at slightly elevated temperatures (cf. Example 14).
Accordingly, the compounds act in the same way as in a solid rubber once the polymer of the latex has precipitated.
The cross-linking reaction also takes place with pure polymer, i.e. there is generally no need for metal oxides (cf. Example 16). Thus, given suitable stabilisation, the well known disadvantage of metal oxides may be avoided, for example in the polychloroprene mixtures.
It has been found that, using TMDHCH (melting point approximately 70.degree. C.), cross-linking reactions take place at room temperature and at slightly elevated temperatures, for example, not only on polychloroprene-mercaptan types, but also on polychloroprene-thiuram types (=sulphur-modified types), cf. Example 17.
This reaction mechanism which, accordingly, also takes place in the case of thiuram types and the dependence upon the degree of oligomerisation may be utilised for largely solving a problem familiar to those skilled in the art, namely the problem of storing sulphur-modified polychloroprenes.
It is well known that the viscosity of the crude polymer (for example Mooney viscosity at 100.degree. C.) is not as stable as that of polychloroprene-mercaptan types, for example. By adding small quantities of monomeric TMDHCH or small quantities of 6-ethocy-TMDHCH, the degredation reaction which normally continues during storage of the sulphur-modified polychloroprene may be arrested or suppressed by controlled pre-cross-linking. This improves the stability of viscosity during storage of the crude polymer (cf. Example 18).
Another surprising feature of this new cross-linking method, preferably using TMDHCH (melting point approximately 70.degree. C.), is that, where the optimal dosage of from 1.5 to 2.5 phr is used, the cross-linking reaction comes to an end and, in the event of so-called "over-vulcanisation", there is virtually no further cross-linking, as is the case where conventional cross-linking systems are used. This is apparent from the trend of the Vulkameter curve, which, on completion of the main cross-linking reaction, runs substantially parallel to the time axis. In some cases, a slight maximum of the shear modulus is even observed. This means that the difference between T.sub.90 and T.sub.80 (time for 90% and 80% vulcanisation) is very small (cf. Example 19).
Technologically, this property is of importance insofar as, where articles of large volume are vulcanised at the conventional vulcanisation temperatures, the outer lays have the same degree of cross-linking as the middle of the vulcanisate which, as any skilled in the art know, improves the dynamic behaviour of the article.
It has been found that the new cross-linking reaction, preferably using TMDHCH (melting point approximately 70.degree. C.), may even be used in combination with conventional accelerators/cross-linking agents, including sulphur and sulphur donors. Despite the fact that the cross-linking velocity and the degree of cross-linking at normal vulcanisation temperatures are influenced, the property of cross-linking at room temperature and at slightly elevated temperatures surprisingly remains intact (cf. Examples 20, 21, 22).
Another feature of this new cross-linking process is that, by comparison with the thioureas generally used hitherto, dynamic crack formation and crack growth behaviour is considerably improved (cf. Example 19).
The cross-linking agents used in accordance with the present invention may be added inquantities familiar to those skilled in the art for cross-linking the polymers containing active halogen.
Quantities of from 0.1 to 15 parts, by weight, per 100 parts by weight, of solid rubber are preferably used for cross-linking, quantities of from 0.3 to 3 parts, by weight, being particularly preferred.
For stabilising the viscosity of and for pre-cross-linking sulphur-modified and nonsulphur-modified polychloroprenes, it is preferred to use quantities of from 0.01 to 1.0 part, by weight, per 100 parts, by weight, of solid rubber.
The compounds used according to the present invention may be used either on their own or even in combination with conventional cross-linking agents and accelerators, particularly thiourea, thiuram/amine, sulphur/thiuram/guanidine, thiazolidine thione, thiadiazine and triazine.
The cross-linking temperature is known to those skilled in the art and is governed by the particular cross-linking process used. Cross-linking is preferably carried out at temperatures between room temperature (i.e. up to about +5.degree. C., depending on climatic and seasonal conditions) and up to +270.degree. C. and, with particular preference, at temperatures of from +40.degree. C. to +200.degree. C.
Examples of suitable vulcanisation processes are press heating, hot-air heating, superheated-steam heating, injection and transfer vulcanisation processes, continuous processes carried out in superheated steam, hot air, infrared heat, hot air/microwaves, salt baths, fluid beds, so-called "Auma" processes for films, rubberised fabrics, sheets, V-belts and drive belts, also lead-jacket processes. The cross-linking agents may also be used at room temperature in the absence of external pressure for a so-called "self-vulcanisation" process.
Combinations of processes may also be used. Thus, pre-cross-linking may be carried out at room temperature or a slightly elevated temperature, followed by further cross-linking at elevated temperature, final cross-linking again being possible at room temperature or a slightly elevated temperature.
Conversely, however, pre-cross-linking may even be carried out at elevated temperature to such a minimal extent that the pre-cross-linked material may still be rolled, i.e. re-used. Final cross-linking may then be carried out in the absence of pressure at room temperature or at slightly elevated temperatures.
Further mixture constituents which may be added to the polymers cross-linkable by the present process, preferably the polychloroprene and the chlorobutyl and bromobutyl rubber, are the conventional constituents normally encountered in the solid rubber, latex and adhesive field, for example, metal oxides, such as zinc oxide, magnesium oxide, calcium oxide or lead oxides, active and inactive carbon blacks and also light fillers, such as silicas, kaolins (cf. Example 23) and chalks, siliceous chalks, plasticisers, antiagers and anti-ozonants, expanding agents and processing aids, such as factice, stearic acid, polyethylene wax, parrafins, resins and vaseline.
Other known polymers may also be added to the polymers cross-linkable by this process, as known to those skilled in the art. Examples of such polymers are NR, IR, SBR, BR, EPM, EPDM, NBR, PVC, styrene, EVAC, CM. PE and PP.
EXAMPLE 1
Production of a polychloroprene mixture is known manner in accordance with the following formulation on mixing rolls:
EXAMPLE 2
EXAMPLE 3
EXAMPLE 4
EXAMPLE 5
EXAMPLE 6
EXAMPLE 7
EXAMPLE 8
A film was cast. Drying and storage for 6 days at 20.degree. C., followed by 1 day at 70.degree. C.
Testing of the melting behaviour of the film under a microscope:
A and B soften at approximately 115.degree. C.
Film A begins to form bubbles at 115.degree. C.
Film B only forms bubbles beyond 160.degree. C.
EXAMPLE 9
EXAMPLE 10
EXAMPLE 11
EXAMPLE 12
The plates of the 2-minute heating stage may be re-plasticised on mixing rolls or in a refiner.
EXAMPLE 13
Cross-linking of adhesive-grade polychloroprene with TMDHCH
EXAMPLE 14
Cross-linking of polychloroprene latex
EXAMPLE 15
EXAMPLE 16
EXAMPLE 17
EXAMPLE 18
EXAMPLE 19
EXAMPLE 20
EXAMPLE 21
EXAMPLE 22
EXAMPLE 23
Claims
I claim:
1. A process for crosslinking polychloroprene by adding crosslinking agents, characterised in that the crosslinking agents used are compounds corresponding to the formulae: ##STR3## wherein R.sub.1 represents hydrogen or C.sub.1 -C.sub.4 alkyl; R.sub.2 represents hydrogen C.sub.1 -C.sub.14 alkyl, C.sub.1 -C.sub.14 alkoxy, C.sub.1 -C.sub.14 alkyl phenyl, phenyl, naphthyl, hydroxyl or C.sub.1 -C.sub.14 alkyl hydroxyl; R.sub.3 and R.sub.4, which may be the same or different, each represents hydrogen or C.sub.1 -C.sub.4 alkyl; R.sub.5 represents hydrogen or C.sub.1 -C.sub.4 alkyl; and R.sub.6 and R.sub.7 which may be the same or different, each represents hydrogen or C.sub.1 -C.sub.4 alkyl; and in that crosslinking is carried out in the conventional way.
2. A process as claimed in claim 1, characterised in that the crosslinking agent is used in quantities of from 0.1 to 15 parts, by weight, per 100 parts, by weight, of solid rubber.
3. A process as claimed in claim 1 characterised in that the crosslinking agent is used in quantities of from 0.3 to 3 parts, by weight, per 100 parts, by weight, of solid rubber.
4. A process as claimed in claim 1 characterised in that crosslinking is carried out at a temperature of from 5.degree. to 270.degree. C.
5. A process as claimed in claim 1 characterised in that crosslinking is carried out at a temperature of from 40.degree. to 200.degree. C.
6. Crosslinked polychloroprene obtained by the process claimed in claim 1.
Patent Citations (8)
| Patent | Date | Inventor | Cited By |
|---|---|---|---|
| US3335124 | 1967-08-01 | Larsen | |
| US3379707 | 1968-04-01 | Lund et al. | |
| US3686154 | 1972-08-01 | Khaa | |
| US3844985 | 1974-10-01 | Fukutani et al. | |
| US3872128 | 1975-03-01 | Byck | |
| US3919143 | 1975-11-01 | Morris | |
| CAX703198 | 1965-02-01 | ||
| FRX1310524 | 1961-07-01 |