US 4,177,172 AGrant
Aqueous Nitrocellulose/Alkyd Resin Dispersion
Issue Date:1979-12-04
•5 Claims
Abstract
Aqueous dispersion of a binder for coating compositions comprising 5-35% by weight of nitrocellulose, 0-30% by weight, based on (a) of plasticizer, 5-50% by weight of alkyd resin, 30-80% by weight of water, 0.5-10% by weight of emulsifier, and optionally 4-40% by weight of a urea resin and/or melamine resin.
Metadata
Assignee
- Bayer Aktiengesellschaft
Inventors
- Hans-Joachim Traenckner
- John Goossens
- Wolfgang Kremer
- Heinz Kronke
Application Information
Application Number:US 9695575
Filing Date:1978-12-14
Priority Date:1977-01-26
Art Unit:143
Classifications
IPC:
C08L 118
Field of Search:
26015;17 R
Patent Drawings
This patent does not have any drawings.
Description
EXAMPLES
In the following parts are parts by weight and % are % by weight.
EXAMPLE A
A solution in ethyl acetate was prepared from 100 g of nitrocellulose chips containing approximately 12% of nitrogen, Standard Specification 24 E in accordance with DIN 53,179, consisting of 82% of collodion cotton and 18% of dibutyl phthalate,
100 g of groundnut oil fatty acid alkyd resin having an oil content of 41%, and
300 g of ethyl acetate.
After stirring slowly for approximately 3 hours a clear solution was obtained which was combined with 300 g of a 3% strength aqueous solution of a partially saponified polyvinyl acetate (molecular weight 40,000, degree of hydrolysis 86-89%), whilst stirring slowly. The mixture was then dispersed for 2 minutes in an Ultra-Turrax type 45 laboratory disperser by raising the speed of rotation continuously to 10,000 revolutions per minute. The solvent was distilled off under reduced pressure. A primary emulsion having a solids content of 41.8% and a viscosity corresponding to a flow time of 34 seconds in the DIN cup No. 4 (DIN 53,211) was thus obtained.
EXAMPLE B (comparison)
A dispersion was prepared as described in Example A, except that instead of the partially saponified polyvinyl acetate, 300 g of an aqueous solution of a non-ionic fatty acid ester (emulsifier Emulphor EL of BASF) were used. This gave an emulsion which was stable for a max. of 3-5 hours and which had an average particle size of 13.mu. in a determination of particle pattern.
EXAMPLE C
A dispersion was prepared from
100 g of groundnut oil fatty acid alkyd resin having an oil content of 41%,
100 g of nitrocellulose chips as in Example A and
300 g of ethyl acetate.
After stirring for 3 hours, a clear solution was obtained which was combined with 500 g of a 2.5% strength solution of a partially saponified polyvinyl acetate (molecular weight 80,000, degree of hydrolysis 86-89%) in water. The procedure described under Example A was then followed. A primary emulsion with a solids content of approximately 30% and a flow viscosity of 28 seconds in the DIN cup No. 4 as then obtained.
USE EXAMPLES
EXAMPLE 1 (comparison test)
A lacquer of the following composition was prepared:
The resulting lacquer exhibited a viscosity corresponding to a flow time of approximately 30 seconds, measured in accordance with DIN 53,211 (DIN cup No. 4). The curing to give films and the assessment are described in Table 1.
EXAMPLE 2
A dispersion of the following composition was prepared:
The resulting dispersion exhibited a viscosity corresponding to a flow time of approximately 15 seconds, measured in accordance with DIN 53,211, DIN-cup 4.
EXAMPLE 3
A lacquer of the following composition was prepared:
Claims
We claim:
1. An aqueous dispersion of a binder for coating compositions said dispersion comprising (a) 5-50% by weight of nitrocellulose, (b) 5-30% by weight, based on (a), of plasticizer for (a), (c) 5-50% by weight of alkyd resin having an oil content of 5-50% by weight, based on alkyd resin, (d) 30-80% by weight of water, and (e) 0.5-10% by weight of emulsifier, the percentages of a, c, d and e being based on the sum of components (a) to (e), in which the emulsifier is a member of the group consisting of (i) a partially saponified polyvinyl acetate having a degree of hydrolysis of 70-97%, (ii) a polyvinyl pyrrolidone, and (iii) a hydrolyzed vinyl acetate/vinyl pyrrolidone copolymer, the particle size of the dispersed phase being from 0.1 to 1.5.mu..
2. An aqueous disperson according to claim 1, containing additionally 4-40% by weight based on components (a) to (e), of a urea and/or melamine resin.
3. An aqueous dispersion according to claim 1, in which the alkyd resin contains 20 to 45% by weight of oil.
4. An aqueous dispersion according to claim 1, in which the dispersed particles have an average size from 0.1 to 0.5.mu..
5. A process for the production of an aqueous dispersion according to claim 1, characterized in that nitrocellulose, alkyd resin and-- optionally-- plasticizer are dissolved in an organic solvent, preferably at room temperature, the alkyd resin and the nitrocellulose amounting to at least 30% by weight of the solution, and this obtained solution is subsequently dispersed into an aqueous solution of the emulsifer, this emulsifier solution amounting to at least one half by weight of the alkyd resin/nitrocellulose/plasticizer solution, and the organic solvent is removed by distillation.
Patent Citations (6)
| Patent | Date | Inventor | Cited By |
|---|---|---|---|
| US2937153 | 1960-05-01 | Rasmussen et al. | |
| US3370025 | 1968-02-01 | Salo et al. | |
| US3450652 | 1969-06-01 | Lin | |
| US3522070 | 1970-07-01 | Webb | |
| US3551367 | 1970-12-01 | Gasper et al. | |
| US3615792 | 1971-10-01 | Keene |