Abstract
Disclosed are flame-retardant thermoplastic resins such as graft ABS, polystyrene, polypropylene, and the like, containing polyethylene tetrabromophthalate and antimony trioxide.
Metadata
Assignee
- Borg-Warner Corporation
Inventors
- Ralph P. Arthur
- Roy M. Turner
Application Information
Application Number:US 790634&
Filing Date:1977-04-25
Priority Date:1977-04-25
Art Unit:142
Classifications
IPC:
C08L 5502C08L 6702C09K 328
Field of Search:
26045.75 B;873
Patent Drawings
This patent does not have any drawings.
Description
Background of the Invention
This invention relates to thermoplastic resins made flame retardant by mixing the resin with brominated polyesters, particularly those prepared from tetrabromophthalic anhydride and low molecular weight glycols such as polyethylene glycol, polybutylene glycol and polypropylene glycol; and antimony trioxide.
The theory and practice of using heavily halogenated organic chemical compounds and antimony oxide as additives to produce flame-retarded thermoplastic compositions is a well-known commercial process. The commonly used, highly brominated aromatic organic compounds result in a number of adverse effects to the thermoplastic flame-retarded products.
These adverse effects are (1) poor efficiency; i.e., high levels of bromine and antimony oxide are required to obtain adequate flame retardancy in thin sections; (2) a drastic reduction of overall balance of physical properties, particularly heat distortion and impact strength; and (3) mold buildup of flame retardant during processing and resultant surface degradation of molded parts.
Summary of the Invention
This invention relates to the use of heavily brominated polyesters as flame retardants in thermoplastic polymers such as graft ABS, polystyrene, polypropylene and the like.
Example 1
A stirred reactor was charged with 930 grams (15 moles) of ethylene glycol. The glycol was stirred and heated to 155.degree. C, and 2320 grams (5 moles) of tetrabromophthalic anhydride was added. The reaction mixture was stirred and heated at 165.degree. C for eight hours to distill off water produced during the reaction to form diester. The reaction was mass cooled to 130.degree. C; 200 grams of xylene were added and excess glycol was azeotroped from the reaction mixture at 170.degree.-175.degree. C; and pressure was then reduced to 20 mm Hg. at 170.degree.-175.degree. C to remove residual xylene and glycol. Analysis of the reaction product at this point gave:
Melting point: 35-50.degree. C; % Br: 55.3; Acid number: 13.0
Infrared analysis: Diester, trace of glycol, no anhydride or carboxyl evident.
500 GRAMS OF THE ABOVE DIESTER (0.87 MOLES) WAS HEATED IN A STIRRED REACTOR TO 145.degree. C and 2.0 grams of Sb.sub.2 O.sub.3 and 0.35 grams of (TNPP) tri-nonylphenyl phosphite was added. Pressure was adjusted to 20 mm Hg. and condensation to polyester (with removal of glycol) was continued for 10 hours at 185.degree. C. Infrared analysis showed the reaction product to be polyethylene tetrabromophthalate: ##STR1##
Analysis Found: Melting point: 105-115.degree. C; % Br: 58.5; Acid number: 8.0; Molecular weight (DMF): 3,000.
Example 2
After formation of the diester of Example 1, the reaction mixture was stirred and heated for 3.5 hours at 195-200.degree. C at 10 mm Hg. pressure to produce a polyethylene tetrabromophthalate with the following analysis:
Melting point: 95-100.degree. C; % Br: 57.5; Acid number: 4.6; Molecular weight (DMF): 1,260.
Example 3
The performance of compositions of this invention were determined by incorporating the flame retardants in various thermoplastic polymers by the following procedure:
Specimens were prepared by mixing the components in a Banbury mixer 3 minutes at 320.degree. F. The composition was sheeted off on a two-roll mill, cooled, ground and compression molded at 300.degree. F to form 1/8 inch (125 mils) or 60 mil test specimens. Testing was by standard ASTM or Borg-Warner Chemicals test methods.
Example 4
To establish the efficiency of the brominated polyester as a flame retardant in ABS polymers, a series of compounds were prepared as in Example 3 with reduced amounts of both brominated polyester compound and antimony trioxide.
Example 5
Due to the surprising efficiency of the brominated polyester flame retardant, further compositions were prepared as in Example 3 with reduced amounts of the brominated polyester.
Example 6
In order to show the efficiency of the brominated polyester/antimony oxide system in other thermoplastic polymers, a series of compositions were prepared in a Banbury mixer, sheeted, ground and compression molded in the same manner as described in Example 2. The results are as follows:
Claims
We claim:
1. A flame-retardant composition comprising (1) 100 parts by weight of a graft ABS resin; (2) from about 10.4 to about 26.7 parts by weight of polyethylene tetrabromophthalate; and (3) from about 4.5 to about 7.5 parts by weight of antimony trioxide.
Patent Citations (5)
| Patent | Date | Inventor | Cited By |
|---|---|---|---|
| US3419518 | 1968-12-01 | Mahling et al. | |
| US3738958 | 1973-06-01 | Paul | |
| US3883481 | 1975-05-01 | Kopetz et al. | |
| US4024102 | 1977-05-01 | Stackman et al. | |
| CAX973830 | 1966-08-01 |
Non-Patent Literature (2)
- Hackh's Chemical Dictionary, Fourth Edition, McGraw-Hill, N.Y., pp. 302 & 303, 1969.
- I & EC Product Research & Development, vol. 8, No. 4, Dec. 1969, pp. 381-391.