A thermally crystallizable glass consisting essentially of 45-57 SiO.sub.2, 29-38 Al.sub.2 O.sub.3, 13-22 Na.sub.2 O, in parts by weight, and the parts totalling 100. For each of these 100 parts, the glass contains 0.5-5 parts of ZrO.sub.2 and 1-10 parts of ZnO. The five constituents constitute at least 95 weight percent of the total glass and a thermally crystallized glass-ceramic article suitable as kitchen ware or table ware is made from this glass.
Metadata
Assignee
- Owens-Illinois, Inc.
Inventors
- Megumi Tashiro
- Masamichi Wada
- Toshio Yamanaka
- Kenichi Tani
Application Information
Application Number:US 1318136
Filing Date:1971-04-06
Priority Date:1965-01-27
Art Unit:115
Classifications
IPC:
C03C 322
Field of Search:
651063339.6;39 DV;52;39.8
Patent Drawings
This patent does not have any drawings.
Description
There are several methods of producing glass-ceramics containing a large amount of Na.sub.2 O. Patent SHO-37-1123 corresponding to U.S. Pat. No. 2,933,857 describes a method in which a glass body containing 0-5% of F by weight is used as a nuclei forming agent. Patent SHO-38-10725 describes a method in which a glass body containing 1-5% by weight of ZnS is used as a nuclei forming agent. Patent SHO-36-16032 describes a method in which 0.08-0.5% by weight of Cr.sub.2 O.sub.3 or at least 6% by weight of titanate of a divalent metallic oxide is used.
However, the present inventors discovered that the following new glasses of limited composition containing SiO.sub.2, Al.sub.2 O.sub.3, Na.sub.2 O as the chief components and ZrO.sub.2 and ZnO as the nuclei forming agent, can be transformed into new and useful glass-ceramics having a high softening temperature and high mechanical strength by thermal crystallization.
This invention in one aspect pertains to a method of manufacturing a glass-ceramic and glass-ceramic articles having a higher softening temperature and a higher mechanical strength than the initial glass, by heat treating a glass body consisting essentially by weight of 45-57 parts SiO.sub.2, 29-38 parts Al.sub.2 O.sub.3, 13-22 parts Na.sub.2 O, and in excess over the 100 parts of the sum of the above components including as a nucleating agent by weight of 0.5 parts to 5 parts ZrO.sub.2 and 1-10 parts ZnO, the total of the above essential components being at least 95% of the glass body, by heating it at the temperature between the annealing point and the softening point of the initial glass, for example, 700.degree.-800.degree. C., to form the crystal nuclei; then the heating is continued with the gradual increase of the temperature, for example, at the increasing rate of 5.degree. C./minute, then by keeping it finally at the temperature of 900.degree.-1150.degree. C. for 0.5-10 hours.
The application of this invention is shown in Table 1.
Batches of glass were prepared so as to have the composition specified in Table 1. These batches of glass were fused for 7-8 hours at a temperature of 1500.degree.-1550.degree. C. in an electric oven. A number of glass rods of each composition were made, about 5 mm. in diameter. The glass rods of Examples 1-11 were kept at a temperature of 800.degree. C. for 2 hours in an electric oven to form the crystal nuclei. After this the rods were further heated at the rate of 5.degree. C./minute up to a temperature of 1100.degree. C., and then held at that temperature for 2 hours in order to increase the amount of fine crystals. The heat treatment was the same for Examples 12-17 except that the second holding temperature was 1050.degree. C. In Example 18 the first holding temperature for 2 hours was 750.degree. C. and the second 2 hour holding temperature was 1000.degree. C.
It was confirmed by the X-ray analysis that the main crystals separated by such thermal crystallization heat treatment were nepheline. The bending strength (modulus of rupture) shown in Table 1 was obtained by measurement with a bending strength measuring device which is supported by 3 points and has a span of 40 mm. The specimens were crystallized rods of about 50 mm. length and 5 mm. diameter.
The reason for limiting the components ZrO.sub.2, SiO.sub.2, Al.sub.2 O.sub.3, ZnO and Na.sub.2 O to a certain percentage is as follows. If ZrO.sub.2 is less than 0.5 parts, the fine-grained glass-ceramic is very difficult to produce, and if ZrO.sub.2 is greater than 5 parts, the liquidus temperature of glass becomes very high, and the molding of glass becomes difficult. Therefore, ZrO.sub.2 must be limited to 0.5-5 parts. If ZnO is less than 1 part or more than 10 parts, the finely crystalline glass-ceramics cannot be produced. Therefore, ZnO must be limited to 1-10 parts. If SiO.sub.2 is less than 45 parts, the chemical resistance of glass-ceramic becomes inferior, and if SiO.sub.2 is more than 57 parts, the thermal crystallization of the glass takes place only with difficulty. Therefore, SiO.sub.2 must be limited to 45-57 parts. If Al.sub.2 O.sub.3 is less than 29 parts, the finely crystallized glass-ceramic cannot be produced, and if Al.sub.2 O.sub.3 is more than 38 parts, the liquidus temperature of the glass becomes high. Therefore, Al.sub.2 O.sub.3 must be limited to 29-38 parts. If Na.sub.2 O is less than 13 parts, the thermal crystallization of the glass takes place with difficulty, and if Na.sub.2 O is more than 22 parts, the finely crystalline glass-ceramic cannot be obtained. Therefore, Na.sub.2 O must be limited to 13-22 parts. Moreover, if the above mentioned SiO.sub.2, Al.sub.2 O.sub.3, Na.sub.2 O, ZrO.sub.2 and ZnO (total) are less than 95% of the glass, softening deformation during the crystallization becomes great. Therefore, according to the invention the sum of SiO.sub.2, Al.sub.2 O.sub.3, Na.sub.2 O, ZrO.sub.2 ZnO contained in the glass is at least 95% by weight.
Glass (and resulting glass-ceramic) compositions of the present invention having the best properties, notably with respect to fineness of crystals and strength, contain at least 3.5 weight percent ZrO.sub.2 or of ZrO.sub.2 plus TiO.sub.2, based on the total glass composition.
Miscellaneous oxides can be added to the compositions of the invention so long as they do not materially affect or alter the basic characteristics of the glasses and the glass-ceramic materials of the invention. For instance, based on 100 parts by weight of SiO.sub.2 + Al.sub.2 O.sub.3 + Na.sub.2 O, up to 3 parts each of Li.sub.2 O, K.sub.2 O, CaO or TiO.sub.2, or less than 3 parts MgO, or less than 2 parts BaO can be included. Also, addition of up to about 2 parts of PbO improves chemical durability and up to about 2 parts of P.sub.2 O.sub.5 reduces the tendency of articles of large cross-sectional area to crack during heat treatment.
According to this invention, since glass-ceramics having a high mechanical strength and a fine structure can be produced economically, the final products are suitable for use as industrial material or for the production of kitchen utensils or tableware.
Claims
We claim:
1. A thermally crystallizable glass consisting essentially of 45-57 parts SiO.sub.2, 29-38 parts Al.sub.2 O.sub.3, 13-22 parts Na.sub.2 O, said parts being based on 100 parts of Sio.sub.2, Al.sub.2 O.sub.3 and Na.sub.2 O, and for each 100 parts of SiO.sub.2, Al.sub.2 O.sub.3 and Na.sub.2 O, 0.5-5 arts of ZrO.sub.2 and 1-10 parts of ZnO, wherein said essential SiO.sub.2, Al.sub.2 O.sub.3, Na.sub.2 O, ZrO.sub.2, and ZnO constituents constitute at least 95 weight percent of the total glass, additionally containing 0-3 parts by weight of TiO.sub.2 for each 100 parts by weight of SiO.sub.2 + Al.sub.2 O.sub.3 + Na.sub.2 O, the total of the weight percent ZrO.sub.2 + the weight percent TiO.sub.2 being at least 3.5 based on the total glass composition, said glass being capable of in situ thermal crystallization to form a glass ceramic containing nepheline crystals.
2. A glass-ceramic containing nepheline crystals formed by thermal crystallization of a glass consisting essentially of in parts by weight 45-57 SiO.sub.2 , 29-38 Al.sub.2 O.sub.3, 13-22 Na.sub.2 O, said parts being based on 100 parts of SiO.sub.2, Al.sub.2 O.sub.3 and Na.sub.2 O, and for each 100 parts of SiO.sub.2, Al.sub.2 O.sub.3 and Na.sub.2 O, 0.5-5 parts of ZrO.sub.2 and 1-10 parts of ZnO, wherein said essential SiO.sub.2, Al.sub.2 O.sub.3, Na.sub.2 O, ZrO.sub.2 and ZnO constituents constitute at least 95 weight percent of the total glass-ceramics, and additionally containing 0-3 parts by weight of TiO.sub.2 for each 100 parts by weight of SiO.sub.2 + Al.sub.2 O.sub.3 + Na.sub.2 O, the total of the weight percent ZrO.sub.2 + the weight percent TiO.sub.2 being at least 3.5, based on the total glass composition.
Patent Citations (14)
| Patent | Date | Inventor | Cited By |
|---|---|---|---|
| US2920971 | 1960-01-01 | Stookey | |
| US3006775 | 1961-10-01 | Chen | |
| US3146114 | 1964-08-01 | Kivlighn | |
| US3201266 | 1965-08-01 | MacDowell | |
| US3236662 | 1966-02-01 | MacDowell | |
| US3252811 | 1966-05-01 | Beall | |
| US3282712 | 1966-11-01 | Tashiro et al. | |
| US3313609 | 1967-04-01 | Megles | |
| US3455706 | 1969-07-01 | Takagi et al. | |
| US3473937 | 1969-10-01 | Tashiro et al. | |
| US3528828 | 1970-09-01 | Smith | |
| US3586521 | 1971-06-01 | Duke | |
| US3720526 | 1973-03-01 | Duke et al. | |
| DT1,099,135 | 1961-01-01 |
Non-Patent Literature (3)
- Vanes-"Crystallization Studies of Na.sub.2 O-Al.sub.2 O.sub.3 -SiO.sub.2 Base Glasses"-Advances in Glass Technology pub. 1962, NYC. Plenum Press, pp. 377-381.
- Leim et al., Phase Diagrams for Ceramists pub. 1964 by J. Amer. Cer. Soc. FIG. 501, System Na.sub.2 O-Al.sub.2 O.sub.3 -SiO.sub.2 .
- J. Ceramic Raw Materials, in Ceramic Industry Magazine, Chicago, 1967, p. 153.