A flexible heat set biaxially oriented film article having in at least one portion thereof a bead type heat seal is prepared by clamping together adjacent the portion to be heat sealed, superimposed plies of a heat set, biaxially oriented polyester film, said film being characterized as having a tensile strength of at least 15,000 psi and a ratio of tensile strengths in the TD to MD direction between about 0.67 and 1.5, imposing a heat energy source to fuse in a bead type seal the superimposed film and maintaining the plies of film pressed together until the source of heat energy is retracted therefrom.
Metadata
Assignee
- Union Carbide Corporation
Inventors
- Howard D. Bassett
- Franklin E. Schrage
- George F. Kirkpatrick
Application Information
Application Number:US 4258606
Filing Date:1973-12-18
Priority Date:1971-10-18
Art Unit:161
Classifications
IPC:
B32B 3126B32B 3128
Field of Search:
15653428272;306;499;82;515;311;25139480
Patent Drawings
This patent does not have any drawings.
Description
Example 1
A "Weldotron" Model W 5222 intermittent radiant heat sealer was employed in this example. This sealer uses film clamping means comprising stationary lower jaws and movable upper jaws that clamp the film therebetween, and a movable radiant heating element that contacts and severs the film to be heat sealed. The radiant sealing element was maintained at a temperaure between about 1200.degree. and 1300.degree.F. and was long enough to completely heat seal the plies of film in one operation.
Polyester polymeric films, 0.0005 inch (1/2 mil) thick, having the properties summarized in Table I below were employed in this example. Flat sheets of film were superimposed one on the other with the machine and transverse directions of each film aligned. Clamps spaced 3/16 inch apart were used to press the plies of film together and provide a band of untensioned film therebetween in which the heat seals were to be formed. Heat seals were formed in both the transverse direction and machine direction, the transverse direction seal was formed perpendicular to the machine direction of the film and the machine direction seal was formed parallel to the machine direction of the film.
The plies of film were fused and severed with each operation of the heat sealin apparatus with parallel, bead like seals being formed along the edges of each adjacent segment of heat sealed film. Samples of the heat sealed film segments were evaluated within 24 hours of preparation and additional samples were aged at 73.degree.F. and 140.degree.F. for varying periods of time. A summary of the seal strength properties of both unaged and aged heat seal film samples is reported in Table II.
The ultimate tensile and seal strength tests reported herein were run in accordance with the test procedure of ASTM D 882-64T using a jaw separation speed of 20 inches/min. An "Instron" tensile test machine was used in these evaluations. The tensile and seal strength properties used throughout the specification and in the claims shall be interpreted according to this test procedure.
Heat seals formed in polyester polymeric film in accordance with the practice of the present invention exhibited high seal strength properties as formed. Heat seals formed in Film B, said film having a TD/MD ratio of 1.0, extracted somewhat better retention of seal strength properties than seals formed in Film A (TD/MD ratio of 1.5) when aged for an extended period at 140.degree.F.
Example 2
A "Weldotron" Model W 2318 continuous radiant heat sealing machine as described, for example, in U.S. Pat. No. 3,243,330 was employed in this example. The following polyester polymeric films were used in this example:
Heat seals formed in Film A and Film B using the continuous radiant heat sealer described above, operating at a temperature between about 1200.degree. and 1500.degree.F. and a clamp spacing of about 1/4 inch, were determined to have the following heat seal strenth:
Example 3
Using the apparatus and procedures of Example 1, the following polyester polymeric films were heat sealed.
Film A -- a heat set biaxially oriented film of intrinsic viscosity of about 0.55 having tensile strengths in the transverse direction of 30,000 psi and in the machine direction of 20,000 psi. The TD/MD ratio was 1.5. The film thickness was 0.00075 inches (0.75 mils).
Film B -- a heat set biaxially oriented polyester film of intrinsic viscosity of about 0.55 having a transverse direction tensile strength of 22,000 psi and machine direction tensile strength of 21,000 psi with the TD/MD ratio being 1.0. The thickness of this film was 0.92 mils.
Film C -- a biaxially oriented shrinkable polyester film having a shrinkage of about 30% at 100.degree.C.
Superimposed plies of each of Film A, Film B and Film C were heat sealed. The original strength (measured within 24 hours of forming) of the seals formed with Film A and Film B are as follows:
Claims
What is claimed is:
1. A method for heat sealing superimposed layers of flexible, biaxially oriented, heat set polyester polymeric films, prepared from polyethylene terephthalic esters including the steps of: a. superimposing a first ply of said flexible, biaxially oriented, heat set polyester polymeric film over a second ply of said polyester film each of said plies of film being characterized as having a tensile strength of at least about 15,000 psi and a ratio of transverse to machine direction tensile strengths between about 0.67 and 1.5; b. clamping a portion of said plies of super-imposed film adjacent to and for at least the length thereof coextensive with the portion to be heat sealed so as to press the first and second plies of said film against each other and maintain the portion of said film to be heat sealed in a substantially untensioned state; c. imposing on the portion of said superimposed plies of film to be heat sealed heat from a heat energy source of sufficient intensity for the time necessary to fuse in a bead type seal the portion of untensioned superimposed film; and d. maintaining said plies of film pressed together until the source of heat energy is retracted therefrom.
2. The method of claim 1 wherein the heat energy source is a radiant heat energy source.
3. The method of claim 2 wherein the radiant heat energy source contacts and severs the portion of film to be heat sealed.
4. The method of claim 1 wherein said superimposed plies of film are fused into separate, adjacent bead type seals.
5. The method of claim 1 wherein said plies of film are characterized as having a ratio of transverse to machine direction tensile strenth between about 0.85 and 1.3.
6. The method of claim 1 wherein said heat energy source is at a temperature of at least about 1100.degree.F.
Patent Citations (7)
| Patent | Date | Inventor | Cited By |
|---|---|---|---|
| US3009851 | 1961-11-01 | Madsen | |
| US3165499 | 1965-01-01 | Alles | |
| US3321353 | 1967-05-01 | Zelnick | |
| US3355337 | 1967-11-01 | Zelnick | |
| US3413175 | 1968-11-01 | Rochla | |
| US3574046 | 1971-04-01 | Buteux | |
| US3736219 | 1973-05-01 | McTaggart |