US 2003/0193042 A1Application
Mixtures comprising thiophene/anion dispersions and certain additives for producing coatings exhibiting improved conductivity, and methods related thereto
Publication Date:2003-10-16
•19 Claims
•8 Drawing Sheets
Abstract
Disclosed are mixtures comprising aqueous thiophene/anion dispersions, such as polythiophene/polystyrene sulfonate aqueous dispersions, and additives, as well as coatings produced therefrom. Coatings produced from these mixtures yield significant improvements in electrical conductivity without the need for a high temperature treatment as compared to coatings produced from unmodified aqueous polythiophene dispersions (e.g., BaytronP) and to coatings produced from state-of the-art aqueous polythiophene-additive mixtures. These conductivity improvements are achieved without detracting from the optical transparency of the coating. Because characteristics of volume resistivity of less than 6.6 ohmcm and optical transmission greater than 80% are important for conductive coating applications, coatings produced from the mixtures of the present invention have significant advantages over coatings produced from the state-of-the-art mixtures in many applications.
Also disclosed are a variety of substrates or articles of manufacture coated with the mixtures of the present invention for use in various applications where a combination of high electrical conductivity, excellent optical transparency and low temperature processing are important, such as electronic and optoelectronic devices.
Metadata
Inventors
- Pin Go
- Dieter Freitag
- John Connell
Application Information
Application Number:US 10/349,285
Filing Date:2003-01-21
Priority Date:2002-01-22
Patent Drawings (8 sheets)
Description
CROSS REFERENCE TO RELATED APPLICATION
[0001] The present application claims the benefit of and priority to U.S. Provisional Application No. 60/350,397, as filed on Jan. 22, 2002.
FIELD OF INVENTION
[0002] The present invention relates generally to electrically conductive organic polymers, more specifically to aqueous mixtures comprising thiophene/anion dispersions and additives, and coatings and articles produced therefrom. These mixtures provide significant improvements in electrical conductivity without detracting from optical transmission and without requiring high temperature thermal treatment.
BACKGROUND
[0003] Conducting polymers (CP's) have received considerable attention in recent years due to their potential applications in a variety of electronic devices. CP's are presently used in commercial products, such as anti-static coatings on plastics, photographic film and electronic packaging materials. Other CP applications include solid electrode capacitors, through-hole plating of printed circuit boards, coatings for cathode ray tubes (to prevent dust attraction), hole injecting layers on indium tin oxide (ITO) substrates for electroluminescent devices, and sensors. Future applications, such as an ITO replacement leading to completely flexible, organic electronic devices, will require improvement in conductivity without sacrificing other properties such as optical transparency.
[0004] A variety of conducting polymers are described in the art, and several are commercially available, such as BaytronP (product of Bayer AG) and Panipol (product of Panipol Ltd.). Of the different CP families, (i.e., polyacetylenes, polyphenylenes, poly(p-phenylenevinylene)s, polypyrroles, polyanilines, and polythiophenes) polythiophenes are arguably the most stable thermally and electronically see, Handbook of Oligio- and Polythiophenes, D. Fichou, Editor, Wiley-VCH, New York (1999), J. Roncali, Chem. Rev., 97, 173 (1997), A. Kraft, A. C. Grimsdale and A. B. Holmes, Angew. Chem., 110, 416 (1998), J. Roncali, J Mater. Chem., 9, 1875 (1999), J. Roncali, Annu. Rep. Prog. Chem. Sec. C., 95, 47 (1999), A. J. Heeger, Synth. Met., 55-57, 3471 (1993) and G. Kobmehl and G. Schopf, Adv. Polym. Sci., 129, 1 (1996). The BaytronP product is a polythiophene/polystyrene sulfonate composition available as an aqueous dispersion containing about 1.3% solids. This aqueous dispersion is typically used to prepare coatings on various substrates. BaytronP is prepared from 3,4-ethylenedioxythiophene (EDT) in aqueous or predominately aqueous media in the presence of polystyrene sulfonic acid (PSS, a dopant) using an oxidant such as iron trichloride see, L. B. Groenendaal, F. Jonas, D. Freitag, H. Pielartzik and J. R. Reynolds, Adv. Mater., 12(7), 481 (2000). Coatings derived from BaytronP have been reported to exhibit a wide range of surface resistance depending upon coating thickness. The surface conductivity of BaytronP, and that of other CP based coatings, will increase with increasing coating thickness while the optical transmission will decrease. In most coating applications, the coatings must exhibit a useable combination of electrical conductivity, optical transparency and environmental stability (i.e., stability to moisture and oxygen). The appropriate balance of these properties is of critical importance; thus a means for improving this balance of properties would represent a significant advancement and enable new applications for these materials.
[0005] One approach to improving the electrical conductivity of polythiophenes has been via the use of additives (see e.g., U.S. Pat. No. 5,766,515). It has been shown that certain additives, when mixed with BaytronP aqueous dispersion and subsequently used to make coatings, can produce an increase in the electrical conductivity (i.e., decrease in surface resistivity); however a high temperature treatment (at about 200 C) is required to realize this improvement. The high temperature treatment is a major disadvantage because certain substrates cannot tolerate such high temperatures.
[0006] No explanation of the mechanism associated with conductivity enhancement is offered in the art; thus it is impossible to elucidate what additives may bring about this increase in electrical conductivity. Although the use of D-sorbitol (a sugar derivative) as an additive to BaytronP is shown in the art as affecting electrical conductivity improvement, the enhancement in conductivity is only realized after shock drying at 200 C. for at least 90 seconds. The reported measured decrease in surface resistance (in the best case) is from about 3500 ohm/square to about 100 ohm/square. Because the coating thickness information for such coatings is not given, the volume resistivity of these coatings cannot be calculated. The high temperature shock drying at 200 C. step limits the use of the additive technology described in the art, as this temperature may exceed the thermal capability or cause deleterious shrinkage of certain plastic substrates. Further, the effects of this additive technology on optical transparency are not available.
SUMMARY OF THE INVENTION
[0007] In view of the above, there is a need to formulate mixtures containing thiophene/anion dispersions and additives for producing coatings that exhibit improved conductivity without decreased optical transparency. There is also a need for a producing such coatings without employing a high temperature heat treatment.
[0008] It is, therefore, an object of the present invention to formulate mixtures comprising thiophene/anion dispersions and additives for producing coatings that exhibit improved conductivity without decreased optical transparency.
[0009] It is another object of the present invention to provide a method for producing such coatings without employing a high temperature heat treatment.
[0010] It is yet another object of the present invention to produce substrates or articles coated with the mixtures comprising thiophene/anion dispersions and additives for use in electronic or optoelectronic devices.
[0011] The present invention pertains to certain additives that, when mixed with thiophene/anion dispersions, particularly polythiophene/polystyrene sulfonate aqueous dispersions, more particularly the commercially available dispersion BaytronP, impart an improved combination of processing characteristics, electrical conductivity and optical transparency into coatings produced therefrom. The improvement in this combination of properties is significant as compared to unmodified BaytronP and to state-of-the-art examples that contain additives (as disclosed in U.S. Pat. No. 5,766,515). The mixtures of the present invention offer significant advantages over the state-of-the-art technology, which thereby make these mixtures more attractive for existing applications and enable new applications. The mixtures of the present invention have a wide spectrum of coating-based applications and allow for the coating of a variety of substrates, including but not limited to, organic polymers, inorganic substrates, and carbon-based substrates. These new mixtures can be fabricated into a variety of material forms, such as coatings, fibers, fabrics, and foams. They can be used, under mild processing temperatures, to render a variety of articles and substrates electrically conductive without affecting optical transparency.
[0012] The above summary of the present invention is not intended to describe each illustrated embodiment or every implementation of the present invention. The figures and the detailed description that follow more particularly exemplify these embodiments.
BRIEF DESCRIPTION OF THE DRAWINGS
[0013] The invention may be more completely understood in consideration of the following detailed description of various embodiments of the invention in connection with the accompanying drawings, in which:
[0014] FIGS. 1A, 1B and 1C illustrate the chemical structures of the preferred additives according to an embodiment of the present invention;
[0015] FIG. 2 graphically illustrates the surface resistance of multiple BaytronP coatings on polycarbonate, coated with a primer, after drying for 5 minutes at 80 C.;
[0016] FIG. 3 graphically illustrates the change in surface resistance as a result of different drying treatments, per FIG. 2 ;
[0017] FIG. 4 graphically illustrates the surface resistance of BaytronP/-butyrolactone coatings, on polycarbonate substrate, according to an embodiment of the present invention; and
[0018] FIG. 5 graphically illustrates the effect of drying conditions on the surface resistance of BaytronP/-butyrolactone coatings, on polycarbonate substrate, according to an embodiment of the present invention.
[0019] While the invention is amenable to various modifications and alternative forms, specifics thereof have been shown by way of example in the drawings and will be described in detail. It should be understood, however, that the intention is not to limit the invention to the particular embodiments described. On the contrary, the intention is to cover all modifications, equivalents, and alternatives falling within the spirit and scope of the invention as defined by the appended claims.
DETAILED DESCRIPTION OF PREFERRED EMBODIMENTS
[0020] The present invention pertains to aqueous mixtures containing a thiophene/anion dispersion and an at least one additive. The term thiophene/anion dispersion, as used herein, refers to a dispersion consisting essentially of an oliogmer, dendrimer or polymer containing thiophene groups in a cationic form with an anionic compound, anionic oligomer, anionic dendrimer or anionic polymer, and water. The term additive, as used herein, describes the species that are combined with a thiophene/anion dispersion, particularly a polythiophene/polystyrene sulfonate aqueous dispersion, more particularly the commercially available dispersion BaytronP, to arrive at mixtures for producing coatings that exhibit a significant improvement in the combination of electrical conductivity and processing characteristics with no decrease in optical transparency as compared to coatings produced from state-of-the-art mixtures. The term state-of-the-art, as used herein, refers to mixtures comprising polythiophene/polystyrene sulfonate aqueous dispersion and an additive (and coatings produced therefrom) as disclosed in U.S. Pat. No. 5,766,515 as this art reference discloses the most advanced technology comprising thiophene/anion aqueous dispersions, especially as pertaining to the polythiophene/polystyrene sulfonate aqueous dispersions, and additives known at this time.
[0021] The improvements in electrical conductivity and processing characteristics of the coatings of the present invention are achieved while using relatively low drying temperatures (from about 80 C. to about130 C.). The present invention overcomes limitations of the state-of-the-art mixtures and coatings produced therefrom by providing a significant improvement in this combination of properties without requiring a high temperature heat treatment.
[0022] BaytronP (available from Bayer AG, Pittsburg, Pa.), based on product literature, consists essentially of poly(3,4-ethylenedioxythiophene) doped with the polyanion of polystyrene sulfonic acid, also referred to as polystyrene sulfonate (PSS), dispersed in aqueous media at a concentration of about 1.2-1.3% solids. Other components, such as wetting agents, leveling agents, surfactants, organic binders, polymeric binders, crosslinking agents, coupling agents and dispersing agents or any combination thereof may also be present in this formulation.
[0023] A variety of additives can be useful in the mixtures of the present invention, and these additives can be added to the thiophene/anion dispersions, such as the commercially available BaytronP polythiophene/polystyrene sulfonate aqueous dispersions, particularly at several different concentrations. The preferred concentrations of the additives used herein are calculated as follows. The BaytronP aqueous dispersion contains 1.3% by weight of polythiophene/polystyrene sulfonate, thus 100 g of BaytronP solution contains 1.3 g of solids. A 1:1 mixture of BaytronP:additive would thus consist of an equal amount, by weight, of polythiophene/polystyrene sulfonate and additive.
[0024] The preferred additives for use herein (see FIG. 1 ) can be classified broadly as cyclo-aliphatic ketals, cyclo-aliphatic lactones, cyclo-aliphatic carbonates, cyclic-oxides, cyclic triketones, anhydrides, aminocarbonic acids, aliphatic monocarbonic acids, phenols and inorganic acids. From each broad class of preferred additives, there are more preferred additives that yield even better results. These more preferred additives give rise to coatings with volume resistivities less than 0.3 ohmcm when dried at only 80 C. for 5 minutes. Examples of more preferred additives include 2,2-dimethyl-1,3-dioxolane, cyclohexanone ethylene ketal, cyclohexanedione mono ethylene ketal, and 2,2-dimethyl-3-methylhydroxy-1,3-dioxolane from the cyclo-aliphatic ketal class (these additives are manufactured by Lancester Synthesis Corp., Windham, N.H.; Fluka Holding AG, Buchs, Switzerland; and Lancester Synthesis Corp., respectively); -valerolactone, -caprolactone and -butyrolactone from the cyclo-aliphatic lactone class (these additives are manufactured by Fluka Holding AG; Dow Chemical Co., Midland, Mich.; and BASF Corp., Hannibal, Mo., respectively); ethylene carbonate from the cyclo aliphatic carbonate class (this additive is manufactured by Fluka Holding AG); styrene oxide and glycidol from cyclic-oxide class (these additives are manufactured by Fluka Holding AG); ninhydrin from the cyclic diketone class (this additive is manufactured by Fluka Holding AG); maleic anhydride, phthalic anhydride, and acetic anhydride from the anhydride class (these additives are manufactured by Fluka Holding AG; BASF Corp.; and Mallinckrodt Baker Inc., Phillipsburg, N.J., respectively); 2-aminobutyric acid and 4-(dimethylamino) butyric acid from the aminocarbonic acid class (this additive is manufactured by Fluka Holding AG) and acetic acid from the aliphatic carbonic acid class (this additive is commercially available from Sigma-Aldrich Corp., San Louis, Mo.); cresols (ortho, meta and para), phenol, 4-hydroxyphenol, and 4- hydroxybenzene sulfonic acid from the phenol class (these additives are manufactured by Sumitomo Chemical America, New York, N.Y.; Mallinckrodt Baker Inc.; Eastman Chemical Co., Kingsport, Tenn.; and Lancester Synthesis Corp., respectively); and phosphoric acid from the inorganic acids class (this additive is manufactured by Mallinckrodt Baker Inc.). The chemical derivatives of these broad classes of functional groups may also be utilized as additives in the mixtures of the present invention. Further, a combination (i.e., more than one) of the preferred additives provided herein or their derivatives may also be utilized in the mixtures of the present invention. Furthermore, the preferred additives, their derivatives, or any combination thereof that are incorporated into an oligomer, a dendrimer or a polymer may also be utilized as additives in the mixtures of the present invention.
[0025] It is contemplated that mixtures of the present invention may comprise other components, such as wetting agents, leveling agents, surfactants, organic binders, polymeric binders, crosslinking agents, coupling agents, dispersing agents, or any combination thereof.
[0026] The mixtures of the present invention can be fabricated into a variety of material forms, such as coatings, fibers, fabrics, and foams. Coatings can be produced from these mixtures using a variety of coating techniques, such as spin coating, spray coating, roll coating or hand drawing or any other common coating technique onto glass or plastic substrates or articles of manufacture. The coatings produced from these mixtures are subsequently dried.
[0027] Substrates or articles of manufacture coated with the mixtures of the present invention may be utilized in a variety of applications, such as in the manufacture of electronic or opto-electronic devices. These applications include the following: touch-screens, organic light emitting diodes (OLED), polymer light emitting diodes (PLED), electrochromic (smart) windows, electrochromic displays, back lights, batteries, sensors, anti-radiation coatings, anti-static coatings, catalysts, electromagnetic shielding, electromechanical actuators, electronic membranes, embedded array antennas, fuel cells, infrared reflectors, photovoltaic (PV) junction devices, non-corrosive paint, non-linear optical devices, conductive paint, polymer electrolytes, capacitors, semiconductor circuits, thin film transistors (TFTs), waveguides, and wires (low current).
[0028] In order to demonstrate the improvements in the desired properties of the coatings of the present invention, direct comparisons with state-of-the-art coatings and with coatings produced from unmodified BaytronP are made and presented herein below. Accordingly, mixtures having various concentrations of BaytronP and D-sorbitol are prepared in accordance to U.S. Pat. No. 5,766,515 in order to produce the state-of-the-art coatings. This state-of-the-art patent is selected for comparison purposes because it is the only one that describes the invention in sufficient detail to reproduce. Coatings subsequently fabricated from these mixtures are characterized for electrical conductivity and optical transmission. Due to the variables associated with these measurements, quantitative comparison for measurements obtained using different devices and different operators can be problematic. Thus, for the purposes of exemplifying the improvements due to the use of the additives disclosed herein, the unmodified BaytronP and the state-of-the-art coatings are compared directly with the coatings prepared from the mixtures of the present invention, with the same operator utilizing the same measurement techniques and devices to carry out the comparisons.
[0029] As the comparisons hereinbelow illustrate, the use of select, especially the preferred additives in the mixtures of the present invention, are instrumental in bringing about the desired property improvements without the need for any high temperature treatments.
[0030] In preparing the mixtures, the additives, in solid or liquid form, are mixed in with BaytronP aqueous dispersion, and allowed to mix for several minutes with minor agitation. The additives are typically completely soluble or miscible with the BaytronP aqueous dispersion. The resulting mixtures are subsequently coated onto a glass or plastic substrate using either a spin coating apparatus or a doctor blade. Typically, a glass substrate (about 2 inches in diameter) is mounted onto the vacuum chuck of the spin coating device. The mixture is added to the center of the substrate, and spinning is initiated. The samples are spun at 2000 revolutions per minute for a period of 10 seconds. The coatings are subsequently dried for 5 minutes at 80 C. The surface resistivity of each coating is measured. Subsequently, the coatings are treated at 200 C. for 90 seconds or 1.5 minutes. The surface resistivity of each coating is measured again to determine the effects of the heat treatment.
[0031] The thickness of each coating prepared for characterization ranges from about 100 nm to about 1000 nm; coatings having thicknesses in the range of about 100 nm to about 300 nm are preferred for use herein. The coatings are characterized for optical transparency/optical transmission, surface resistance, and volume resistivity, which is calculated using the following equation:
[0032] Wherein tthe coating thickness, measured in centimeters (cm), k is the geometrical correction factor. The constant k is related to the coating thickness, probe spacing and sample size.
[0033] The characterization data for coatings produced from the state-of-the-art mixtures, i.e., BaytronP/D-sorbitol mixtures at several different concentrations, is presented in Table 1. For comparative purposes, the characterization results for the coating produced from BaytronP dispersion without any additive (i.e., unmodified BaytronP) is also presented in Table 1. It is concluded, from the information in Table 1 and from information in U.S. Pat. No. 5,766,515, that the most significant improvement in conductivity (i.e., lowest volume resistivity) that is exhibited by the BaytronP/D-sorbitol mixture is achieved only after a high temperature treatment at 200 C. The high temperature treatment can be disadvantageous because it limits the substrates upon which coatings with improved electrical conductivity can be applied. In particular, certain polymeric substrates, such as bisphenol A polycarbonate (PC) and poly(ethylene terephthalate) (PET), cannot be used with this state-of-the-art mixture for the very reason. Both PC and PET have thermal stabilities far below 200 C., as measured by their glass transition temperatures. For many conductive coating applications, it is desirable to coat inexpensive plastic substrates, such as PET and PC, in a continuous, rapid and automated process.
| TABLE 1 | |||||
|---|---|---|---|---|---|
| BaytronP/D-Sorbitol Coating Characterization on Glass | |||||
| Mixture | Surface | Volume | |||
| BaytronP: | Thickness | Resistivity | Resistivity | Drying | |
| D-Sorbitol | (nm) | (k-ohm/square) | pH | (ohm cm) | Conditions |
| 1:1 | 190 | 105 | 2 | 37.9 | RT, 12 hr |
| 1:2 | 210 | 112 | 2 | 44.6 | RT, 12 hr |
| 1:6 | 240 | 53 | 2 | 24.1 | RT, 4 hr |
| 1:12 | 260 | 52 | 2 | 25.7 | RT, 12 hr |
| 1:1 | 190 | 65 | 2 | 23.4 | 200 C., |
| 1.5 min | |||||
| 1:12 | 260 | 13.4 | 2 | 6.6 | 200 C., |
| 1.5 min | |||||
| Mixture | Surface | Volume | |||
| Unmodified | Thickness | Resistivity | Resistivity | Drying | |
| BaytronP | (nm) | (k-ohm/square) | pH | (ohm cm) | Conditions |
| 1:0 | 85 | 160 | 2 | 26.0 | 80 C., |
| 5 min | |||||
| RT room temperature, about 23 C. | |||||
[0034] Achieving volume resistivities of less than 0.3 ohmcm, down to 0.037 when dried at only 80 C. for 5 minutes, represent a major improvement as compared to the volume resistivities of unmodified BaytronP coatings (two orders of magnitude improvement) and of the BaytronP/D-sorbitol coatings (1-2 orders of magnitude improvement). Even compared to the BaytronP/D-sorbitol coating that is shock-dried at 200 C. and that yields the best results of all state-of-the-art-art coatings, the coatings of the present invention still exhibit greater than a twenty-fold reduction in volume resistivity. This improvement in conductivity is achieved with no sacrifice in optical transparency. The use of the additives described herein, in combination with the significant reduction in temperature treatment, provide for coatings (of the present invention) with a significant advantage over the state-of-the-art coatings.
| TABLE 2 | |||||
|---|---|---|---|---|---|
| BaytronP/2,2-Dimethyl-1,3-Dioxolane Coating | |||||
| Characterization on Glass | |||||
| Mixture | |||||
| BaytronP: | Thick- | Surface | Volume | Drying | |
| 2,2-Dimethyl-1,3- | ness | Resistivity | Resistivity | Con- | |
| Dioxolane | (nm) | (k-ohm/square) | pH | (ohm cm) | ditions |
| 1:1 | 160 | 8.9 | 2 | 2.70 | 80 C., |
| 5 min | |||||
| 1:6 | 160 | 0.67 | 2 | 0.20 | 80 C., |
| 5 min | |||||
| 1:10 | 150 | 0.65 | 2 | 0.18 | 80 C., |
| 5 min | |||||
| 1:20 | 150 | 0.52 | 2 | 0.15 | 80 C., |
| 5 min | |||||
| 1:50 | 150 | 7.6 | 2 | 2.16 | 80 C., |
| 5 min | |||||
[0035] Coatings produced from BaytronP/2,2-Dimethyl-1,3-dioxolane mixtures provide a significant improvement in electrical conductivity relative to the unmodified BaytronP and BaytronP/D-sorbitol coatings. This improvement is achieved with considerably lower drying temperatures. Based on solids content, the concentrations of the components are 1 part BaytronP and between 6 and 20 parts 2,2-dimethyl-1,3-dioxolane. The relevant data is presented in Table 2. Further heating of these coatings, to 200 C. for 1.5 minutes, provides no significant enhancement in electrical conductivity. Coatings produced from BaytronP/cyclohexanone ethylene ketal mixtures provide a significant improvement in electrical conductivity even when a lower temperature drying cycle is utilized. Based on solids content, the concentrations of the components are 1 part BaytronP and 10 parts cyclohexanone ethylene ketal. The relevant data is presented in Table 3. Further heating of these coatings, to 200 C. for 1.5 minutes, provides no significant enhancement in electrical conductivity.
| TABLE 3 | |||||
|---|---|---|---|---|---|
| BaytronP/Cyclohexanone Ethylene Ketal | |||||
| Coating Characterization on Glass | |||||
| Mixture | |||||
| BaytronP: | Thick- | Surface | Volume | Drying | |
| Cyclohexanone | ness | Resistivity | Resistivity | Con- | |
| Ethylene Ketal | (nm) | (k-ohm/square) | pH | (ohm cm) | ditions |
| 1:1 | 180 | 44.2 | 2 | 15.06 | 80 C., |
| 5 min | |||||
| 1:10 | 150 | 0.89 | 2 | 0.25 | 80 C., |
| 5 min | |||||
[0036] Coatings produced from BaytronP/cyclohexanedione mono ethylene ketal mixtures, at 1:1 and 1:6 BaytronP to cyclohexanedione mono ethylene ketal concentrations, also provide a significant improvement in electrical conductivity. The relevant data is presented in Table 4. Heating of these BaytronP/cyclohexanedione mono ethylene ketal coatings, to 200 C. for 1.5 minutes, provides only a slight enhancement in electrical conductivity. For example, the first entry in Table 4 shows a reduction in volume resistivity from 0.96 to 0.69 after this thermal treatment.
| TABLE 4 | |||||
|---|---|---|---|---|---|
| BaytronP/Cyclohexanedione Mono Ethylene Ketal | |||||
| Coating Characterization on Glass | |||||
| Mixture | |||||
| BaytronP: | |||||
| Cyclohex- | |||||
| anedione | Thick- | Surface | Volume | Drying | |
| Mono Ethylene | ness | Resistivity | Resistivity | Con- | |
| Ketal | (nm) | (k-ohm/square) | pH | (ohm cm) | ditions |
| 1:1 | 280 | 1.8 | 2 | 0.96 | 80 C., |
| 5 min | |||||
| 1:6 | 280 | 2.82 | 2 | 1.50 | 80 C., |
| 5 min | |||||
[0037] Coatings produced from BaytronP/2,2-dimethyl-3-methylhydroxy-1,3-dioxolane mixtures, preferably having BaytronP:2,2-dimethyl-3-methylhydroxy-1,3-dioxolane concentrations of about 1:6 to about 1:20, provide a significant improvement in electrical conductivity. The relevant data is presented in Table 5. Further heat treatment of these coatings, for 1.5 minutes at 200 C., provides no improvement in electrical conductivity.
[0038] All coatings produced from BaytronP/:cyclic aliphatic ketal mixtures exhibit optical transparencies similar to that of BaytronP/D-sorbitol coatings and unmodified BaytronP coatings.
| TABLE 5 | |||||
|---|---|---|---|---|---|
| BaytronP/2,2-Dimethyl-3-Methylhydroxy-1,3-Dioxolane Coating | |||||
| Characterization on Glass | |||||
| Mixture | |||||
| BaytronP: | |||||
| 2,2-Dimethyl-3- | Thick- | Surface | Volume | Drying | |
| Methylhydroxy- | ness | Resistivity | Resistivity | Con- | |
| 1,3-Dioxolane | (nm) | (k-ohm/square) | pH | (ohm cm) | ditions |
| 1:1 | 150 | 20.1 | 2 | 5.72 | 80 C., |
| 5 min | |||||
| 1:6 | 170 | 1.69 | 2 | 0.54 | 80 C., |
| 5 min | |||||
| 1:10 | 180 | 1.01 | 2 | 0.345 | 80 C., |
| 5 min | |||||
| 1:20 | 150 | 0.86 | 2 | 0.245 | 80 C., |
| 5 min | |||||
| 1:100 | 90 | 32.5 | 2 | 5.55 | 80 C., |
| 5 min | |||||
[0039] Regarding the cyclo-aliphatic lactone class of additives, the characterization data for coatings produced from BaytronP/-valerolactone, BaytronP/-caprolactone, and BaytronP/-butyrolactone mixtures are presented in Tables 6, 7 and 8, respectively.
[0040] For -valerolactone, the preferred concentration range is from about 1:1 to about 2:1, with the range of about 1:1 to about 1:50 providing the greatest improvement in electrical conductivity. Further heating of these coatings, to 200 C. for 1.5 minutes, provides no additional improvement in electrical conductivity.
| TABLE 6 | |||||
|---|---|---|---|---|---|
| BaytronP/-Valerolactone Coating Characterization on Glass | |||||
| Mixture | Thick- | Surface | Volume | Drying | |
| BaytronP: | ness | Resistivity | Resistivity | Con- | |
| -Valerolactone | (nm) | (k-ohm/square) | pH | (ohm cm) | ditions |
| 1:1 | 150 | 2.42 | 2 | 0.69 | 80 C., |
| 5 min | |||||
| 1:6 | 130 | 1.54 | 2 | 0.38 | 80 C., |
| 5 min | |||||
| 1:10 | 130 | 1.71 | 2 | 0.42 | 80 C., |
| 5 min | |||||
| 1:50 | 120 | 3.1 | 2 | 0.71 | 80 C., |
| 5 min | |||||
| 1:100 | 120 | 10.8 | 2 | 2.46 | 80 C., |
| 5 min | |||||
| 2:1 | 160 | 17.5 | 2 | 5.31 | 80 C., |
| 5 min | |||||
[0041] For -caprolactone, the preferred concentration range is from about 1:1 to about 1:100 BaytronP to -caprolactone. The concentration of 2:1 BaytronP to -caprolactone also provides some improvement. The best results are obtained from the concentration range of about 1:1 to about 1:50. Additional heating of these coatings, to 200 C. for 1.5 minutes, provides no significant increase in electrical conductivity.
| TABLE 7 | |||||
|---|---|---|---|---|---|
| BaytronP/-Caprolactone Coating Characterization on Glass | |||||
| Mixture | Thick- | Surface | Volume | Drying | |
| BaytronP: | ness | Resistivity | Resistivity | Con- | |
| -Caprolactone | (nm) | (k-ohm/square) | pH | (ohm cm) | ditions |
| 1:1 | 180 | 1.55 | 2 | 0.53 | 80 C., |
| 5 min | |||||
| 1:6 | 180 | 1.42 | 2 | 0.48 | 80 C., |
| 5 min | |||||
| 1:10 | 170 | 1.3 | 2 | 0.42 | 80 C., |
| 5 min | |||||
| 1:50 | 140 | 2.6 | 2 | 0.69 | 80 C., |
| 5 min | |||||
| 1:100 | 120 | 8.3 | 2 | 1.89 | 80 C., |
| 5 min | |||||
| 2:1 | 180 | 14.3 | 2 | 4.89 | 80 C., |
| 5 min | |||||
[0042] For -butyrolactone, the preferred concentration range of BaytronP to -butyrolactone is in the range from about 1:1 to about 1:100. Some improvement in electrical conductivity is also realized with the 2:1 concentration. The most preferred concentration range is from about 1:1 to about 1:50. The subsequent heating of these coatings, to 200 C. for 1.5 minutes, provides no significant increase in electrical conductivity.
| TABLE 8 | |||||
|---|---|---|---|---|---|
| BaytronP/-Butyrolactone Coating Characterization on Glass | |||||
| Mixture | Thick- | Surface | Volume | Drying | |
| BaytronP: | ness | Resistivity | Resistivity | Con- | |
| -Butyrolactone | (nm) | (k-ohm/square) | pH | (ohm cm) | ditions |
| 1:1 | 200 | 1.13 | 2 | 0.43 | 80 C., |
| 5 min | |||||
| 1:6 | 180 | 1.31 | 2 | 0.45 | 80 C., |
| 5 min | |||||
| 1:10 | 180 | 1.5 | 2 | 0.51 | 80 C., |
| 5 min | |||||
| 1:50 | 150 | 2.8 | 2 | 0.80 | 80 C., |
| 5 min | |||||
| 1:100 | 130 | 8.8 | 2 | 2.17 | 80 C., |
| 5 min | |||||
| 2:1 | 180 | 36.4 | 2 | 12.43 | 80 C., |
| 5 min | |||||
[0043] All coatings produced from BaytronP:cyclic aliphatic lactone mixtures exhibit optical transparencies similar to that of BaytronP/D-sorbitol coatings and unmodified BaytronP coatings.
[0044] Regarding the cyclo aliphatic carbonate class of additives, coatings produced from BaytronP/ethylene carbonate mixtures are characterized. The characterization data for these coatings are presented in Table 9. The preferred concentration range of this additive is the range from about 1:1 to about 1:50 BaytronP to ethylene carbonate. This entire concentration range provides a significant improvement in electrical conductivity. Further heating of these coatings, to 200 C. for 1.5 minutes, provides no significant improvement in electrical conductivity.
| TABLE 9 | |||||
|---|---|---|---|---|---|
| BaytronP/Ethylene Carbonate Coating Characterization on Glass | |||||
| Mixture | |||||
| BaytronP: | Surface | Volume | |||
| Ethylene | Thickness | Resistivity | Resistivity | Drying | |
| Carbonate | (nm) | (k-ohm/square) | pH | (ohm cm) | Conditions |
| 1:1 | 130 | 1.81 | 2 | 0.45 | 80 C., |
| 5 min | |||||
| 1:6 | 180 | 1.33 | 2 | 0.45 | 80 C., |
| 5 min | |||||
| 1:10 | 190 | 1.28 | 2 | 0.46 | 80 C., |
| 5 min | |||||
| 1:50 | 190 | 2.53 | 2 | 0.91 | 80 C., |
| 5 min | |||||
| 2:1 | 170 | 55.0 | 2 | 17.74 | 80 C., |
| 5 min | |||||
[0045] All coatings produced from BaytronP:ethylene carbonate mixtures exhibit optical transparencies similar to that of BaytronP:D-sorbitol coatings and unmodified BaytronP coatings.
[0046] Regarding the cyclic-oxide class of additives, coatings prepared from BaytronP/styrene oxide and BaytronP/glycidol mixtures are characterized. Characterization data for these coatings is presented in Tables 10 and 11, respectively.
[0047] For the styrene oxide containing coatings, concentrations of 1:10 (BaytronP to styrene oxide) does not provide homogenous solutions. The most preferred concentration is 1:1 because it provides the greatest improvement in electrical conductivity of the cyclic oxide class. Further drying of the 1:1 coating, at 200 C. for 1.5 minutes; does not improve their electrical conductivity.
[0048] Table 10. BaytronP/Styrene Oxide Coating Characterization on Glass
| TABLE 10 | |||||
|---|---|---|---|---|---|
| BaytronP/Styrene Oxide Coating Characterization on Glass | |||||
| Mixture | |||||
| BaytronP: | Surface | Volume | |||
| Styrene | Thickness | Resistivity | Resistivity | Drying | |
| Oxide | (nm) | (k-ohm/square) | pH | (ohm cm) | Conditions |
| 1:1 | 190 | 0.34 | 2 | 0.12 | 80 C., |
| 5 min | |||||
[0049] For the glycidol coatings, concentrations of about 1:1 to about 1:100 (BaytronP to glycidol) are preferred, with the more preferred concentration range being from about 1:1 to about 1:10. Further drying of these coatings, at 200 C. for 1.5 minutes, does not improve their electrical conductivity.
| TABLE 11 | |||||
|---|---|---|---|---|---|
| BaytronP/Glycidol Coating Characterization on Glass | |||||
| Mixture | Thick- | Surface | Volume | ||
| BaytronP: | ness | Resistivity | Resistivity | Drying | |
| Glycidol | (nm) | (k-ohm/square) | pH | (ohm cm) | Conditions |
| 1:1 | 180 | 2.1 | 2 | 0.72 | 80 C., |
| 5 min | |||||
| 1:10 | 180 | 1.55 | 3-4 | 0.53 | 80 C., |
| 5 min | |||||
| 1:100 | 130 | 14.6 | 5 | 3.602 | 80 C., |
| 5 min | |||||
[0050] All coatings produced from BaytronP:cyclic oxide mixtures exhibit optical transparencies similar to that of BaytronP:D-sorbitol coatings and unmodified BaytronP coatings.
[0051] Regarding the cyclic diketone class of additives, coatings prepared from BaytronP/ninhydrin mixtures are characterized. Characterization data for these BaytronP/ninhydrin coatings is presented in Table 12. The concentrations of about 1:1 to about 1:6 and 2:1 (BaytronP to ninhydrin) are preferred as they yield significant improvements in electrical conductivity. Further drying of these coatings, at 200 C. for 1.5 minutes, does not improve their electrical conductivity.
[0052] The coatings produced from BaytronP/ninhydrin mixtures exhibit optical transparencies similar to that of BaytronP/D-sorbitol coatings and unmodified BaytronP coatings.
[0053] Table 12. BaytronP/Ninhydrin Coating Characterization on Glass
| TABLE 12 | |||||
|---|---|---|---|---|---|
| BaytronP/Ninhydrin Coating Characterization on Glass | |||||
| Mixture | Surface | Volume | |||
| BaytronP: | Thickness | Resistivity | Resistivity | Drying | |
| Ninhydrin | (nm) | (k-ohm/square) | pH | (ohm cm) | Conditions |
| 1:1 | 200 | 0.65 | 2 | 0.25 | 80 C., |
| 5 min | |||||
| 1:6 | 190 | 0.7 | 2 | 0.25 | 80 C., |
| 5 min | |||||
| 2:1 | 170 | 1.1 | 2 | 0.35 | 80 C., |
| 5 min | |||||
[0054] Regarding the anhydride class of additives (cyclic and linear), coatings produced from BaytronP/maleic anhydride, BaytronP/phthalic anhydride, and BaytronP/acetic anhydride mixtures are characterized. Characterization data for these coatings is presented in Tables 13, 14 and 15, respectively.
[0055] For maleic anhydride, the preferred concentrations of BaytronP to maleic anhydride is from about 1:1 to about 1:6 and 2:1. Coatings prepared from these mixtures provide significant improvement in electrical conductivity. However, the concentration of 1:6 (BaytronP to maleic anhydride) yields the most significant improvement. As is the case with nearly all of the additives described herein, heat treatment of these coatings, at 200 C. for 1.5 minutes, does not significantly change the electrical conductivity of these coating.
| TABLE 13 | |||||
|---|---|---|---|---|---|
| BaytronP/Maleic Anhydride Coating Characterization on Glass | |||||
| Mixture | |||||
| BaytronP: | Surface | Volume | |||
| Maleic | Thickness | Resistivity | Resistivity | Drying | |
| Anhydride | (nm) | (k-ohm/square) | pH | (ohm cm) | Conditions |
| 1:1 | 180 | 1.6 | 2 | 0.55 | RT, 2 hr |
| 80 C., | |||||
| 5 min | |||||
| 1:2 | 180 | 1.7 | 2 | 0.60 | 80 C., |
| 5 min | |||||
| 1:6 | 180 | 0.5 | 2 | 0.17 | 80 C., |
| 5 min | |||||
| 2:1 | 160 | 2.46 | 2 | 0.75 | 80 C., |
| 5 min | |||||
[0056] For phthalic anhydride, the preferred concentration is about 1:1 (BaytronP to phthalic anhydride). Further heat treatment of these coatings, at 200 C. for 1.5 minutes, does not significantly change the electrical conductivity.
| TABLE 14 | |||||
|---|---|---|---|---|---|
| BaytronP/Phthalic Anhydride Coating Characterization on Glass | |||||
| Mixture | |||||
| BaytronP: | Surface | Volume | |||
| Phthalic | Thickness | Resistivity, | Resistivity, | Drying | |
| Anhydride | (nm) | (k-ohm/square) | pH | ohm cm | Conditions |
| 1:1 | 180 | 1.96 | 2 | 0.67 | 80 C., |
| 5 min | |||||
[0057] For acetic anhydride, the preferred concentration of the BaytronP/acetic anhydride coatings range from about 1:1 to about 1:100, with the most preferred concentration range being from about 1:6 to about 1:100. Heat treatment of these coatings, at 200 C. for 1.5, minutes does not significantly change the electrical conductivity.
[0058] The coatings produced from BaytronP/anhydride (cyclic and linear) mixtures exhibit optical transparencies similar to that of BaytronP/D-sorbitol coatings and unmodified BaytronP coatings.
| TABLE 15 | |||||
|---|---|---|---|---|---|
| BaytronP/Acetic Anhydride Coating Characterization on Glass | |||||
| Mixture | |||||
| BaytronP: | Surface | Volume | |||
| Acetic | Thickness | Resistivity | Resistivity | Drying | |
| Anhydride | (nm) | (k-ohm/square) | pH | (ohm cm) | Conditions |
| 1:1 | 160 | 26.6 | 2 | 8.08 | 80 C., |
| 5 min | |||||
| 1:6 | 160 | 6.5 | 2 | 1.97 | 80 C., |
| 5 min | |||||
| 1:12 | 150 | 1.57 | 2 | 0.45 | 80 C., |
| 5 min | |||||
| 1:50 | 150 | 1.8 | 2 | 0.51 | 80 C., |
| 5 min | |||||
| 1:100 | 140 | 5.3 | 2 | 1.41 | 80 C., |
| 5 min | |||||
[0059] Regarding the aminocarbonic acid and aliphatic carbonic acid classes of additives, coatings prepared from BaytronP/2-aminobutyric acid, BaytronP/4-(dimethylamino)butyric acid, and BaytronP/acetic acid mixtures are characterized. Characterization data for these coatings is presented in Tables 16, 17 and 18, respectively.
[0060] For 2-aminobutyric acid, the preferred concentration range of BaytronP to 2-aminobutyric acid is from about 1:1 to about 1:6, with 1:6 being the most preferred. Further heating, to 200 C. for 1.5 minutes, of the 1:1 coating increases the electrical conductivity of the coating, with the volume resistivity decreasing from 2.01 ohmcm to 0.68 ohmcm.
| TABLE 16 | |||||
|---|---|---|---|---|---|
| BaytronP/2-Aminobutyric Acid Coating Characterization on Glass | |||||
| Mixture | |||||
| BaytronP: | |||||
| 2-Amino- | Surface | Volume | |||
| butyric | Thickness | Resistivity | Resistivity | Drying | |
| Acid | (nm) | (k-ohm/square) | pH | (ohm cm) | Conditions |
| 1:1 | 180 | 5.9 | 2 | 2.01 | 80 C., |
| 5 min | |||||
| 1:6 | 180 | 2.2 | 2 | 0.68 | 80 C., |
| 5 min | |||||
[0061] For 4-(dimethylamino)butyric acid, the preferred concentration range of BaytronP to 4-(dimethylamino)butyric acid is from about 1:1 to about 1:6, with 1:6 being the most preferred. No significant enhancement in electrical conductivity is observed after heating the coatings to 200 C. for 1.5 minutes.
| TABLE 17 | |||||
|---|---|---|---|---|---|
| BaytronP/4-(Dimethylamino)butyric Acid | |||||
| Coating Characterization on Glass | |||||
| Mixture | |||||
| BaytronP: | |||||
| 4-(Dimethyl- | Surface | Volume | |||
| amino) | Thickness | Resistivity | Resistivity | Drying | |
| butyric Acid | (nm) | (k-ohm/square) | pH | (ohm cm) | Conditions |
| 1:1 | 130 | 6.6 | 2 | 1.63 | 80 C., |
| 5 min | |||||
| 1:6 | 140 | 2.6 | 2 | 0.69 | 80 C., |
| 5 min | |||||
[0062] The coatings produced from BaytronP/aminocarbonic acid mixtures exhibit optical transparencies similar to that of BaytronP/D-sorbitol coatings and unmodified BaytronP coatings.
[0063] For acetic acid, the preferred concentration range for BaytronP:acetic acid is from about 1:1 to about 1:100, with the most preferred concentration range being from about 1:12 to about 1:100. No significant enhancement in electrical conductivity is observed after heating the coatings to 200 C. for 1.5 minutes.
| TABLE 18 | |||||
|---|---|---|---|---|---|
| BaytronP/Acetic Acid Coating Characterization on Glass | |||||
| Mixture | Surface | Volume | |||
| BaytronP: | Thickness | Resistivity | Resistivity | Drying | |
| Acetic Acid | (nm) | (k-ohm/square) | pH | (ohm cm) | Conditions |
| 1:1 | 150 | 78.1 | 2 | 22.23 | 80 C., |
| 5 min | |||||
| 1:6 | 160 | 11.0 | 2 | 3.34 | 80 C., |
| 5 min | |||||
| 1:12 | 130 | 3 | 2 | 0.74 | 80 C., |
| 5 min | |||||
| 1:50 | 130 | 4.8 | 2 | 1.18 | 80 C., |
| 5 min | |||||
| 1:100 | 130 | 4.7 | 2 | 1.16 | 80 C., |
| 5 min | |||||
[0064] The coatings produced from BaytronP/acetic acid mixtures exhibit optical transparencies similar to that of BaytronP/D-sorbitol coatings and unmodified BaytronP coatings.
[0065] Regarding the phenol class of additives, coatings prepared from BaytronP/phenol mixtures are characterized. Characterization data for these coatings is presented in Table 19. The preferred concentration range of BaytronP to phenol is from about 1:1 to about 1:4. This class of additives yields highly favorable results. Drying these coatings for 1.5 minutes at 200 C. provides a slight improvement in conductivity. These coatings exhibit optical transparencies similar to that of BaytronP/D-sorbitol coatings and unmodified BaytronP coatings.
| TABLE 19 | |||||
|---|---|---|---|---|---|
| BaytronP/Phenol Coating Characterization on Glass | |||||
| Mixture | Surface | Volume | |||
| BaytronP: | Thickness | Resistivity | Resistivity | Drying | |
| Phenol | (nm) | (k-ohm/square) | pH | (ohm cm) | Conditions |
| 1:1 | 190 | 0.68 | 2 | 0.27 | 80 C., |
| 5 min | |||||
| 1:2 | 210 | 0.38 | 2 | 0.15 | 80 C., |
| 5 min | |||||
| 1:4 | 220 | 0.28 | 2 | 0.12 | 80 C., |
| 5 min | |||||
| 2:1 | 190 | 28.4 | 2 | 10.2 | 80 C., |
| 5 min | |||||
| 1:50 | 130 | 4.8 | 2 | 1.18 | 80 C., |
| 5 min | |||||
| 1:100 | 130 | 4.7 | 2 | 1.16 | 80 C., |
| 5 min | |||||
[0066] For 4-hydroxyphenol (hydroquinone), another phenol, coatings produced from BaytronP/4-hydroxyphenol mixtures are characterized. Characterization data for these coatings is presented in Table 20. The preferred concentration of BaytronP to 4-hydroxyphenol is from about 1:1 to about 1:2. Drying these coatings for 1.5 minutes at 200 C. provides a slight improvement in conductivity. These coatings exhibit optical transparencies similar to that of BaytronP/D-sorbitol coatings and unmodified BaytronP coatings.
| TABLE 20 | |||||
|---|---|---|---|---|---|
| BaytronP/4-Hydroxyphenol Coating Characterization on Glass | |||||
| Mixture | |||||
| BaytronP: | Surface | Volume | |||
| 4-Hydroxy- | Thickness | Resistivity | Resistivity | Drying | |
| phenol | (nm) | (k-ohm/square) | pH | (ohm cm) | Conditions |
| 1:1 | 210 | 0.46 | 2 | 0.183 | 80 C., |
| 5 min | |||||
| 1:2 | 150 | 1.57 | 2 | 0.42 | 80 C., |
| 5 min | |||||
[0067] For 4-hydroxybenzene sulfonic acid, another phenol, coatings prepared from BaytronP/4-hydroxybenzene sulfonic acid mixtures are characterized. Characterization data for these coatings is presented in Table 21. The preferred concentration of BaytronP to 4-hydroxybenzene sulfonic acid is from about 1:1 to about 1:4. Drying these coatings for 1.5 minutes at 200 C. provides a slight improvement in conductivity. These coatings exhibit optical transparencies similar to that of BaytronP/D-sorbitol coatings and unmodified BaytronP coatings.
| TABLE 21 | |||||
|---|---|---|---|---|---|
| BaytronP/4-Hydroxybenzene Sulfonic Acid | |||||
| Coating Characterization on Glass | |||||
| Mixture | |||||
| BaytronP: | |||||
| 4-Hydroxy- | Thick- | Surface | Volume | ||
| benzene | ness | Resistivity | Resistivity | Drying | |
| Sulfonic Acid | (nm) | (k-ohm/square) | pH | (ohm cm) | Conditions |
| 1:1 | 60 | 0.327 | 2 | 0.037 | 80 C., |
| 5 min | |||||
| 1:4 | 90 | 0.428 | 2 | 0.073 | 80 C., |
| 5 min | |||||
[0068] For m-cresol, another phenol, coatings produced from BaytronP/m-cresol mixtures are characterized. Characterization data for these coatings is presented in Table 22. The preferred concentration of BaytronP to m-cresol is from about 1:1 to about 1:6. The coatings produced from this concentration range yield excellent results. Thus, it is conceivable that both higher and lower amounts of m-cresol would yield comparable results. Drying these coatings for 1.5 minutes at 200 C. provides no significant improvement in conductivity. These coatings exhibit optical transparencies similar to that of BaytronP/D-sorbitol coatings and unmodified BaytronP coatings.
| TABLE 22 | |||||
|---|---|---|---|---|---|
| BaytronP/m-Cresol Coating Characterization on Glass | |||||
| Mixture | Surface | Volume | |||
| BaytronP: | Thickness | Resistivity | Resistivity | Drying | |
| m-Cresol | (nm) | (k-ohm/square) | pH | (ohm cm) | Conditions |
| 1:1 | 100 | 0.336 | 2 | 0.064 | 80 C., |
| 5 min | |||||
| 1:4 | 100 | 0.354 | 2 | 0.067 | 80 C., |
| 5 min | |||||
| 1:6 | 100 | 0.38 | 2 | 0.072 | 80 C., |
| 5 min | |||||
[0069] Regarding the inorganic acids class of additives, coatings prepared from BaytronP/phosphoric acid mixtures are characterized. Characterization data for these coatings is presented in Table 22. The highly preferred concentration range of BaytronP to phosphoric acid is from about 1:1 to about 1:10; coatings produced from mixtures in this concentration range yield excellent results. Drying these coatings for 1.5 minutes at 200 C. provides no improvement in conductivity. These coatings exhibit optical transparencies similar to that of BaytronP/D-sorbitol coatings and unmodified BaytronP coatings.
| TABLE 23 | |||||
|---|---|---|---|---|---|
| BaytronP/Phosphoric Acid Coating Characterization on Glass | |||||
| Mixture | |||||
| BaytronP: | Thick- | Surface | Volume | ||
| Phosphoric | ness | Resistivity | Resistivity | Drying | |
| Acid | (nm) | (k-ohm/square) | pH | (ohm cm) | Conditions |
| 1:1 | 160 | 0.58 | 2 | 0.176 | 80 C.,5 min |
| 1:6 | 160 | 0.62 | 2 | 0.188 | 80 C.,5 min |
| 1:10 | 150 | 0.70 | 2 | 0.199 | 80 C.,5 min |
[0070] The surface resistance (in Mega ohms/square) of multiple representative BaytronP coatings is presented in FIG. 2 . These coatings are each prepared on a PC substrate that has been treated with a surface primer to aid in wetting. The coatings are subsequently dried for 5 minutes at 80 C. and their surface resistance is measured. As demonstrated herein, the reproducibility of this data is good, with the surface resistance ranging from 2.8 to 3.6 Mega ohms/square. The effect of higher temperature treatment is presented in FIG. 3 . These coatings exhibit a minor decrease in surface resistance after two drying cycles, and a more significant decrease after heating at 200 C. for 1.5 minutes.
[0071] In order to demonstrate the improved conductivity (i.e., reduction in surface resistance) of the coatings produced from the mixtures of the present invention, relative to the BaytronP coatings illustrated in FIGS. 2 and 3 , BaytronP/-butyrolactone (at a concentration of 1:2) coatings are prepared in the same manner and at the same thickness on a pretreated (with the same primer and dried for 5 minutes at 80 C.) PC substrate. The results for multiple repetitions are presented in FIG. 4 . The decrease in surface resistance due to the use -butyrolactone is very significant because the drop from about 3 Mega ohms/square to about 0.67 kilo ohms/square represents a reduction of over 3000 fold. This effect appears to be independent of the substrate as it has been demonstrated on glass (see, Table 8) and plastic (see, FIGS. 4 and 5 ) substrates.
[0072] The results of the effect of various drying conditions on the surface resistance of the BaytronP/-butyrolactone coating are presented in FIG. 5 . The same drying conditions as used for the unmodified BaytronP coatings are utilized (see FIG. 3 ). The BaytronP/-butyrolactone coatings do not exhibit a significant change in surface resistance, as compared to the coatings presented in FIG. 3 , due to the high temperature treatment.
EXAMPLES
[0073] Having generally described the invention, a more complete understanding thereof can be obtained by reference to the following examples that are provided for purposes of illustration only and do not limit the invention.
Example 1
[0074] Preparation of Comparative Example of BaytronP/D-Sorbitol Coatings
[0075] Four different concentrations of BaytronP/D-sorbitol aqueous mixtures were prepared, in accordance to U.S. Pat. No. 5,766,515, by adding the appropriate amount of D-sorbitol to BaytronP aqueous dispersion. The D-sorbitol was added as a solid and mixed for several minutes at room temperature. The BaytronP:D-sorbitol mixtures were prepared at concentrations of 1:1, 1:2, 1:6 and 1:12 by weight.
[0076] The following procedures were followed for each of the examples described herein (i.e., Examples 1-23). The concentration of each component in the mixture is based on the amount of poly(3,4-ethylenedioxy)thiophene/PSS in the BaytronP dispersion and the selected ratio of the components. The acidity of the resulting mixture is measured using pH indicator paper. The mixture is subsequently used to produce thin coatings via a spin casting technique. The coatings are dried under different conditions. The surface resistivity, in ohms/square, of each coating is measured using a Keithley 2000 four-point probe according to ASTM standards. The thickness of each coating is measured with a stylus (Dek Tek I). The volume resistivity of each coating is calculated using the following equation:
[0077] Wherein tthe coating thickness, measured in centimeters (cm), kthe geometrical correction factor. The constant k is related to the coating thickness, probe spacing and sample size. The optical transmission of the coatings are determined using a UV-Vis near IR spectrophotometer (Varian Model 2200). In some cases, optical transmission is determined using a BYK Gardner Haze-Gard Plus instrument.
[0078] The coatings are treated at 200 C. for 90 seconds or 1.5 minutes. The surface resistivity of each coating is measured before and after this high temperature treatment to determine the effects of the heat treatment.
[0079] The relevant data for this example is presented in Table 1 hereinabove.
Example 2
[0080] Preparation of BaytronP/2,2-Dimethyl-1,3-Dioxolane Coatings
[0081] Five different concentrations of BaytronP/2,2-dimethyl-1,3-dioxolane aqueous mixtures were prepared by adding the appropriate amount of 2,2-dimethyl-1,3-dioxolane to BaytronP aqueous dispersion. The 2,2-dimethyl-1,3-dioxolane was added dropwise, and mixed for several minutes at room temperature. The BaytronP:2,2-dimethyl-1,3-dioxolane mixtures were prepared at concentrations of 1:1, 1:6, 1:10, 1:20 and 1:50 by weight.
[0082] The relevant data for this example is presented in Table 2 hereinabove.
Example 3
[0083] Preparation of BaytronP/Cyclohexanone Ethylene Ketal Coatings
[0084] Two different concentrations of BaytronP/cyclohexanone ethylene ketal aqueous mixtures were prepared by adding the appropriate amount of cyclohexanone ethylene ketal to BaytronP aqueous dispersion. The cyclohexanone ethylene ketal was added dropwise, and mixed for several minutes at room temperature. The BaytronP: cyclohexanone ethylene ketal mixtures were prepared at concentrations of 1:1 and 1:10 by weight.
[0085] The relevant data for this example is presented in Table 3 hereinabove.
Example 4
[0086] Preparation of BaytronP/Cyclohexanedione Mono Ethylene Ketal Coatings
[0087] Two different concentrations of BaytronP/cyclohexanedione mono ethylene ketal aqueous mixtures were prepared by adding the appropriate amount of cyclohexanedione mono ethylene ketal to BaytronP aqueous dispersion. The cyclohexanedione mono ethylene ketal was added dropwise, and mixed for several minutes at room temperature. The BaytronP:cyclohexanedione mono ethylene ketal mixtures were prepared at concentrations of 1:1 and 1:6 by weight.
[0088] The relevant data for this example is presented in Table 4 hereinabove.
Example 5
[0089] Preparation of 2,2-Dimethyl-3-Methylhydroxy-1,3-Dioxolane Coatings
[0090] Five different concentrations of BaytronP/2,2-dimethyl-3-methylhydroxy-1,3-dioxolane aqueous mixtures were prepared by adding the appropriate amount of 2,2-dimethyl-3-methylhydroxy-1,3-dioxolane to BaytronP aqueous dispersion. The 2,2-dimethyl-3-methylhydroxy-1,3-dioxolane was added dropwise and mixed for several minutes at room temperature. The BaytronP:2,2-dimethyl-3-methylhydroxy-1,3-dioxolane mixtures were prepared at concentrations of 1:1, 1:6, 1:10, 1:20 and 1:100 by weight.
[0091] The relevant data for this example is presented in Table 5 hereinabove.
Example 6
[0092] Preparation of BaytronP/-Valerolactone Coatings
[0093] Six different concentrations of BaytronP/-valerolactone aqueous mixtures were prepared by adding the appropriate amount of -valerolactone to BaytronP aqueous dispersion. The -valerolactone was added dropwise, and mixed for several minutes at room temperature. The BaytronP:-valerolactone mixtures were prepared at concentrations of 1:1, 1:6, 1:10, 1:50, 1:100 and 2:1 by weight.
[0094] The relevant data for this example is presented in Table 6 hereinabove.
Example 7
[0095] Preparation of BaytronP/-Caprolactone Coatings Six different concentrations of BaytronP/-caprolactone aqueous mixtures were prepared by adding the appropriate amount of -caprolactone to BaytronP aqueous dispersion. The -caprolactone was added dropwise, and mixed for several minutes at room temperature. The BaytronP:-caprolactone mixtures were prepared at concentrations of 1:1, 1:6, 1:10, 1:50, 1:100 and2:1 by weight
[0096] The relevant data for this example is presented in Table 7 hereinabove.
Example 8
[0097] Preparation of BaytronP/-Butyrolactone Coatings
[0098] Six different concentrations of BaytronP/-Butyrolactone aqueous mixtures were prepared by adding the appropriate amount of -butyrolactone to BaytronP aqueous dispersion. The -butyrolactone was added dropwise, and mixed for several minutes at room temperature. The BaytronP:-butyrolactone mixtures were prepared at concentrations of 1:1, 1:6, 1:10, 1:50, 1:100and2:1 by weight.
[0099] The relevant data for this example is presented in Table 8 hereinabove.
Example 9
[0100] Preparation of BaytronP/Ethylene Carbonate Coatings
[0101] Five different concentrations of BaytronP/ethylene carbonate aqueous mixtures were prepared by adding the appropriate amount of ethylene carbonate to BaytronP aqueous dispersion. The ethylene carbonate was added as a solid and mixed for several minutes at room temperature. The BaytronP:ethylene carbonate mixtures were prepared at concentrations of 1:1, 1:6, 1:10, 1:50 and 2:1 by weight.
[0102] The relevant data for this example is presented in Table 9 hereinabove.
Example 10
[0103] Preparation of BaytronP/Styrene Oxide Coating
[0104] One concentration of BaytronP/styrene oxide aqueous mixtures was prepared by adding the appropriate amount of styrene oxide to BaytronP aqueous dispersion. The styrene oxide was added dropwise, and mixed for several minutes at room temperature. The BaytronP:styrene oxide mixtures were prepared at concentrations of 1:1 by weight.
[0105] The relevant data for this example is presented in Table 10 hereinabove.
Example 11
[0106] Preparation of BaytronP/Glycidol Coatings
[0107] Three different concentrations of BaytronP/glycidol aqueous mixtures were prepared by adding the appropriate amount of glycidol to BaytronP aqueous dispersion. The glycidol was added dropwise, and mixed for several minutes at room temperature. The BaytronP:glycidol mixtures were prepared at concentrations of 1:1, 1:10 and 1:100 by weight.
[0108] The relevant data for this example is presented in Table 11 hereinabove.
Example 12
[0109] Preparation of BaytronP/Ninhydrin Coatings
[0110] Three different concentrations of BaytronP/ninhydrin aqueous mixtures were prepared by adding the appropriate amount of ninhydrin to BaytronP aqueous dispersion. The ninhydrin was added as a solid and mixed for several minutes at room temperature. The BaytronP:ninhydrin mixtures were prepared at concentrations of 1:1, 1:6 and 2:1 by weight.
[0111] The relevant data for this example is presented in Table 12 hereinabove.
Example 13
[0112] Preparation of BaytronP/Maleic Anhydride Coatings
[0113] Four different concentrations of BaytronP/maleic anhydride aqueous mixtures were prepared by adding the appropriate amount of maleic anhydride to BaytronP aqueous dispersion. The maleic anhydride was added as a solid and mixed for several minutes at room temperature. The BaytronP:maleic anhydride mixtures were prepared at concentrations of 1:1, 1:2, 1:6 and 2:1 by weight.
[0114] The relevant data for this example is presented in Table 13 hereinabove.
Example 14
[0115] Preparation of BaytronP/Phthalic Anhydride Coatings
[0116] One concentration of BaytronP/phthalic anhydride aqueous mixture was prepared by adding the appropriate amount of phthalic anhydride to BaytronP aqueous dispersion. The phthalic anhydride was added as a solid and mixed for several minutes at room temperature. The BaytronP:phthalic anhydride mixture was prepared at a concentration of 1:1 by weight.
[0117] The relevant data for this example is presented in Table 14 hereinabove.
Example 15
[0118] Preparation of BaytronP/Acetic Anhydride Coatings
[0119] Five different concentrations of BaytronP/acetic anhydride aqueous mixtures were prepared by adding the appropriate amount of acetic anhydride to BaytronP aqueous dispersion. The acetic anhydride was added dropwise, and mixed for several minutes at room temperature. The BaytronP:acetic anhydride mixtures were prepared at concentrations of 1:1, 1:6, 1:12, 1:50 and 1:100 by weight.
[0120] The relevant data for this example is presented in Table 15 hereinabove.
Example 16
[0121] Preparation of Baytron P/Aminobutyric Acid Coatings
[0122] Two different concentrations of BaytronP/aminobutyric acid aqueous mixtures were prepared by adding the appropriate amount of aminobutyric acid to BaytronP aqueous dispersion. The aminobutyric acid was added as a solid and mixed for several minutes at room temperature. The BaytronP:aminobutyric acid mixtures were prepared at concentrations of 1:1 and 1:6 by weight.
[0123] The relevant data for this example is presented in Table 16 hereinabove.
Example 17
[0124] Preparation of BaytronP/4-(Dimethylamino)butyric Acid Coatings
[0125] Two different concentrations of BaytronP/4-(dimethylamino)butyric acid aqueous mixtures were prepared by adding the appropriate amount of 4-(dimethylamino)butyric acid to BaytronP aqueous dispersion. The 4-(dimethylamino)butyric acid was added as a solid and mixed for several minutes at room temperature. The BaytronP:4-(dimethylamino)butyric acid mixtures were prepared at concentrations of 1:1 and 1:6 by weight.
[0126] The relevant data for this example is presented in Table 17 hereinabove.
Example 18
[0127] Preparation of BaytronP/Acetic Acid Coatings
[0128] Five different concentrations of BaytronP/acetic acid aqueous mixtures were prepared by adding the appropriate amount of acetic acid to BaytronP aqueous dispersion. The acetic acid was added dropwise, and mixed for several minutes at room temperature. The BaytronP:acetic acid mixtures were prepared at concentrations of 1:1, 1:6, 1:12, 1:50 and 1:100 by weight.
[0129] The relevant data for this example is presented in Table 18 hereinabove.
Example 19
Preparation of BaytronP/Phenol Coatings
[0130] Six different concentrations of BaytronP/phenol aqueous mixtures were prepared by adding the appropriate amount of phenol to BaytronP aqueous dispersion. The phenol was added as a solid and mixed for several minutes at room temperature. The BaytronP:phenol mixtures were prepared at concentrations of 1:1, 1:2, 1:4, 1:50, 1:100 and 2:1 by weight.
[0131] The relevant data for this example is presented in Table 19 hereinabove.
Example 20
[0132] Preparation of BaytronP/4-Hydroxypheonol Coatings
[0133] Two different concentrations of BaytronP/4-hydroxypheonol aqueous mixtures were prepared by adding the appropriate amount of 4-hydroxypheonol to BaytronP aqueous dispersion. The 4-hydroxypheonol was added as a solid and mixed for several minutes at room temperature. The BaytronP:4-hydroxypheonol mixtures were prepared at concentrations of 1:1 and 1:2 by weight.
[0134] The relevant data for this example is presented in Table 20 hereinabove.
Example 21
[0135] Preparation of BaytronP/4-Hydroxybenzene Sulfonic Acid Coatings
[0136] Two different concentrations of BaytronP/4-hydroxybenzene sulfonic acid aqueous mixtures were prepared by adding the appropriate amount of 4-hydroxysulfonic acid to BaytronP aqueous dispersion. The 4-hydroxybenzene sulfonic acid was added as a solid and mixed for several minutes at room temperature. The BaytronP 4-hydroxybenzene sulfonic acid mixtures were prepared at concentrations of 1:1 and 1:4 by weight.
[0137] The relevant data for this example is presented in Table 21 hereinabove.
Example 22
[0138] Preparation of BaytronP/m-Cresol Coatings
[0139] Three different concentrations of BaytronP/m-cresol aqueous mixtures were prepared by adding the appropriate amount of m-cresol to BaytronP aqueous dispersion. The m-cresol was added dropwise, and mixed for several minutes at room temperature. The BaytronP:m-cresol mixtures were prepared at concentrations of 1:1, 1:4 and 1:6 by weight.
[0140] The relevant data for this example is presented in Table 22 hereinabove.
Example 23
[0141] Preparation of BaytronP/Phosphoric Acid Coatings
[0142] Three different concentrations of BaytronP/phosphoric acid aqueous mixtures were prepared by adding the appropriate amount of phosphoric acid to BaytronP aqueous dispersion. The phosphoric acid was added dropwise, and mixed for several minutes at room temperature. The BaytronP:phosphoric acid mixtures were prepared at concentrations of 1:1, 1:6 and 1:10 by weight.
[0143] The relevant data for this example is presented in Table 23 hereinabove.
[0144] As noted above, the present invention pertains to aqueous thiophene/anion dispersions comprising additives, and coatings and applications related thereto. The present invention should not be considered limited to the particular examples described above, but rather should be understood to cover all aspects of the invention as fairly set out in the appended claims. Various modifications, equivalent processes, as well as numerous structures to which the present invention may be applicable will be readily apparent to those of skill in the art to which the present invention is directed upon review of the present specification.
Claims
1. A mixture, comprising:
(A) a dispersion consisting essentially of an oliogmer, dendrimer or polymer containing thiophene groups in a cationic form with an anionic compound, anionic oligomer, anionic dendrimer or anionic polymer, and water; and
(B) at least one additive that comprises one or more species of the following functional groups: ketal, lactone, carbonate, cyclic oxide, diketone, anhydride, aminocarbonic acid, carbonic acid, phenol and inorganic acid; and one or more species of the derivates of these functional groups.
2. A mixture according to claim 1, wherein Component A is a dispersion consisting essentially of polythiophene and the polyanion of polystyrene sulfonic acid, and water.
3. A mixture according to claim 1, wherein Component A is a dispersion consisting essentially of poly(3,4-ethylenedioxythiophene) and the polyanion of polystyrene sulfonic acid, and water.
4. A mixture according to claim 1, wherein the ratio of Component A (not including the water) to Component B ranges from about 2:1 to about 1:100 by weight.
5. A mixture according to claim 1, wherein Component B is 2,2-dimethyl-1,3-dioxolane, cyclohexanone ethylene ketal, cyclohexanedione mono ethylene ketal and 2,2-dimethyl-3-methylhydroxy-1,3-dioxolane, -valerolactone, -caprolactone and -butyrolactone, ethylene carbonate, styrene oxide, glycidol, ninhydrin, maleic anhydride, phthalic anhydride, acetic anhydride, 2-aminobutyric acid, 4-(dimethylamino)butyric acid, acetic acid, o-cresol, m-cresol, p-cresol, phenol, 4-hydroxyphenol, 4-hydroxybenzene sulfonic acid, phosphoric acid, or any combination thereof.
6. A coating, fiber, fabric, or foam produced from the mixture according to claim 1.
7. A coating according to claim 6, wherein the coating exhibits a volume resistivity less than 6.6 ohmcm after drying for about 5 minutes at about 80 C.
8. A coating according to claim 6, wherein the coating exhibits a volume resistivity less than 0.5 ohmcm after drying for about 5 minutes at about 80 C.
9. A coating according to claim 6, wherein the coating exhibits a volume resistivity less than 6.6 ohmcm and an optical transmission greater than 80% after drying for about 5 minutes at about 80 C.
10. A coating according to claim 6, wherein the coating exhibits a volume resistivity less than 0.09 ohmcm after drying for about 5 minutes at about 80 C.
11. A flexible substrate or article of manufacture coated with a coating according to claim 6.
12. A coated flexible substrate or article of manufacture according to claim 11, wherein the flexible substrate or article of manufacture comprises a polymeric material.
13. A coated flexible substrate or article of manufacture according to claim 12, wherein the flexible polymeric substrate or article of manufacture is polycarbonate or polyester.
14. A rigid substrate or article of manufacture coated with the coating of claim 6.
15. A coated rigid substrate or article of manufacture according to claim 14, wherein the rigid substrate or article of manufacture comprises glass.
16. An electronic or an optoelectronic device comprising a flexible substrate or article of manufacture according to claim 11.
17. An electronic or an optoelectronic device comprising a rigid substrate or article of manufacture according to claim 14.
18. An electronic or an optoelectronic device according to claim 16, wherein the electronic or optoelectronic device is a touch-screen, organic light emitting diode (OLED), polymer light emitting diode (PLED), electrochromic (smart) window, electrochromic display, back light, battery, sensor, anti-radiation coating, anti-static coating, catalyst, electromagnetic shielding, electromechanical actuator, electronic membrane, embedded array antenna, fuel cell, infrared reflector, photovoltaic (PV) junction device, non-corrosive paint, non-linear optical device, conductive paint, polymer electrolyte, capacitor, semiconductor circuit, thin film transistor (TFT), waveguide, or wire (low current).
19. An electronic or an optoelectronic device according to claim 17, wherein the electronic or optoelectronic device is a touch-screen, organic light emitting diode (OLED), polymer light emitting diode (PLED), electrochromic (smart) window, electrochromic display, back light, battery, sensor, anti-radiation coating, anti-static coating, catalyst, electromagnetic shielding, electromechanical actuator, electronic membrane, embedded array antenna, fuel cell, infrared reflector, photovoltaic (PV) junction device, non-corrosive paint, non-linear optical device, conductive paint, polymer electrolyte, capacitor, semiconductor circuit, thin film transistor (TFT), waveguide, or wire (low current).